A three-dimensional current collector and its preparation method and application, a lithium metal negative electrode and its application
By using nickel-cobalt double metal cyanide in a three-dimensional current collector as the lithium metal anode material in lithium-ion batteries, the problems of lithium dendrites and volume expansion are solved, and the cycle stability and energy density of lithium batteries are improved.
Patent Information
- Application Number
- CN202211719063.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-30
AI Technical Summary
During the repeated charging and discharging process of lithium-ion batteries, lithium dendrites are generated on the surface of the lithium metal anode, which leads to short circuit of the positive and negative electrodes of the battery and reduced cycle stability. The metal lithium anode is prone to volume expansion, affecting the service life of the battery.
A three-dimensional current collector is used, including a fiber base layer with a three-dimensional porous structure and nickel-cobalt double metal cyanide loaded in the fiber base layer. It is prepared by a static aging method to form a nanocubic structure of nickel-cobalt double metal cyanide as a lithium metal negative electrode. material to inhibit the growth and volume expansion of lithium dendrites.
Effectively inhibits the generation of lithium dendrites, improves the cycle stability and energy density of lithium batteries, and extends the service life of the battery.
Smart Images

Figure CN115986133B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries, and specifically relates to a three-dimensional current collector and a preparation method and application thereof, and a lithium metal negative electrode and application thereof. Background Art
[0002] Lithium-ion batteries have been widely used in smart phones, wearable devices, electric vehicles and other fields, and have become an important part of people's daily life. In recent years, the graphite negative electrode of lithium-ion batteries has been greatly affected by its theoretical capacity (372mAh g -1 ) limitations, its specific energy is difficult to increase significantly, so it is imperative to develop the next generation of lithium battery systems.
[0003] Lithium metal is the lightest metal (0.534 g·cm -3 ), its theoretical capacity is 3860mAh·g -1 , which is about 10 times that of a graphite negative electrode, significantly improving the energy density of lithium batteries. However, during the repeated charge and discharge process of lithium metal batteries, a large number of lithium dendrites will form on the negative electrode surface. The sharp lithium dendrites continue to grow and can pierce the separator, causing a short circuit between the positive and negative electrodes of the battery, and in severe cases, causing the battery to explode. At the same time, during the cycle, the metal lithium negative electrode is prone to volume expansion, which ultimately leads to a decrease in the battery's cycle stability. Summary of the Invention
[0004] The purpose of the present invention is to provide a three-dimensional current collector and its preparation method and application, a lithium metal negative electrode and its application. Applying the three-dimensional current collector provided by the present invention to a lithium battery can inhibit the formation of lithium dendrites, alleviate the volume expansion of the lithium metal negative electrode, and improve the cycle stability of the lithium battery.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a three-dimensional current collector, comprising a fiber substrate and nickel-cobalt double metal cyanide loaded in the fiber substrate;
[0007] The fiber base layer has a three-dimensional porous structure;
[0008] The nickel-cobalt double metal cyanide has a cubic structure.
[0009] Preferably, the loading amount of the nickel-cobalt double metal cyanide is 0.5 to 2 mg·cm -2 .
[0010] The present invention also provides a method for preparing the three-dimensional current collector described in the above technical solution, comprising the following steps:
[0011] mixing a soluble nickel salt, a chelating agent, hexacyanocobaltate, and water to obtain a precursor solution;
[0012] The fiber substrate is immersed in the precursor solution and subjected to static aging to obtain the three-dimensional current collector.
[0013] Preferably, the soluble nickel salt includes one or more of nickel nitrate, nickel acetate and sulfate;
[0014] The chelating agent includes one or more of citrate, phosphate and aminocarboxylic acid chelating agents.
[0015] Preferably, the molar ratio of the soluble nickel salt, the chelating agent and the hexacyanocobaltate is (0.6-0.8): (0.6-0.9): (0.2-0.6);
[0016] The molar concentration of hexacyanocobaltate in the precursor solution is 5 to 15 mmol / L.
[0017] Preferably, the mixing comprises:
[0018] first mixing a soluble nickel salt, a chelating agent and a portion of water to obtain a first mixed solution;
[0019] mixing the hexacyanocobaltate and the remaining water for a second time to obtain a hexacyanocobaltate solution;
[0020] The first mixed solution and the hexacyanocobaltate solution are mixed for a third time.
[0021] Preferably, the temperature of the static aging is room temperature, and the time is 18 to 24 hours.
[0022] The present invention also provides a lithium metal negative electrode, comprising a current collector and metallic lithium deposited on the current collector;
[0023] The current collector is the three-dimensional current collector described in the above technical solution or the three-dimensional current collector prepared by the preparation method described in the above technical solution.
[0024] Preferably, the mass ratio of the current collector to metallic lithium is 1:0.76-1.52.
[0025] The present invention also provides the use of the three-dimensional current collector described in the above technical solution, the three-dimensional current collector prepared by the preparation method described in the above technical solution, or the lithium metal negative electrode described in the above technical solution in a lithium ion battery.
[0026] The present invention provides a three-dimensional current collector comprising a fiber substrate and a nickel-cobalt double metal cyanide loaded on the fiber substrate; the fiber substrate has a three-dimensional porous structure; and the nickel-cobalt double metal cyanide has a cubic structure. The present invention introduces a nickel-cobalt double metal cyanide having a cubic structure into a fiber substrate having a three-dimensional porous structure, and utilizes the unique morphological structure and mechanical properties of the nickel-cobalt double metal cyanide to form a composite flexible substrate with large pores. The lithium affinity and electrical conductivity of the nickel-cobalt double metal cyanide result in a low overpotential for lithium deposition thereon, uniform deposition, and the ability to suppress lithium dendrites even at high current densities. Compared to bimetallic compounds such as NiFe, MnFe, and MnCo, the present invention has better electrode stabilization and dendrite growth suppression capabilities, thereby further alleviating the volume expansion of the lithium metal negative electrode and improving the cycle stability of the lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 SEM images of carbon cloth used in the examples and comparative examples of the present invention;
[0028] Figure 2 This is an SEM image of the three-dimensional current collector obtained in Comparative Example 1;
[0029] Figure 3 This is an SEM image of the three-dimensional current collector obtained in Comparative Example 2;
[0030] Figure 4 This is an SEM image of the three-dimensional current collector obtained in Example 1;
[0031] Figure 5 This is an SEM image of the three-dimensional current collector obtained in Example 2;
[0032] Figure 6 This is an SEM image of nickel-cobalt double metal cyanide on the three-dimensional current collector obtained in Example 1;
[0033] Figure 7 This is the XRD pattern of the three-dimensional current collector obtained in Example 1;
[0034] Figure 8 This is a cycle performance diagram of the battery in Test Example 3;
[0035] Figure 9 This is a cycle performance diagram of the battery in Test Example 4;
[0036] Figure 10 This is a diagram of the cycle performance of the battery in Test Example 5. DETAILED DESCRIPTION
[0037] The present invention provides a three-dimensional current collector, comprising a fiber substrate and nickel-cobalt double metal cyanide loaded in the fiber substrate;
[0038] The fiber base layer has a three-dimensional porous structure;
[0039] The morphology of the nickel-cobalt double metal cyanide is a nano cubic structure.
[0040] In the present invention, the chemical formula of the nickel-cobalt double metal cyanide is [Ni3Co(CN)6]·12H2O. In the present invention, the nickel-cobalt double metal cyanide is preferably a solid structure. In the present invention, the side length of the nanocubic structure is preferably 164 nm.
[0041] In the present invention, the loading amount of the nickel-cobalt double metal cyanide is preferably 0.5 to 2 mg·cm -2 , more preferably 0.8 to 1.8 mg·cm -2 , more preferably 1.0 to 1.5 mg·cm -2 .
[0042] In the present invention, the fiber base layer preferably includes carbon cloth, facial mask paper or non-woven fabric.
[0043] The present invention also provides a method for preparing the three-dimensional current collector described in the above scheme, comprising the following steps:
[0044] mixing a soluble nickel salt, a chelating agent, hexacyanocobaltate, and water to obtain a precursor solution;
[0045] The fiber substrate is immersed in the precursor solution and subjected to static aging to obtain the three-dimensional current collector.
[0046] In the present invention, unless otherwise specified, all raw materials are commercially available products well known to those skilled in the art.
[0047] The present invention mixes soluble nickel salt, a chelating agent, hexacyanocobaltate and water to obtain a precursor solution.
[0048] In the present invention, the soluble nickel salt preferably includes one or more of nickel nitrate, nickel acetate, and sulfate. In the present invention, the nickel nitrate is preferably added in the form of nickel nitrate hexahydrate; and the nickel sulfate is preferably added in the form of nickel sulfate heptahydrate.
[0049] In the present invention, the chelating agent preferably includes one or more of citrate, phosphate and aminocarboxylic acid chelating agents. In the present invention, the citrate preferably includes one or more of sodium citrate, ferrous citrate and ferric citrate.
[0050] In the present invention, the hexacyanocobaltate preferably includes one or more of potassium hexacyanocobaltate, silver hexacyanocobaltate and ammonium hexacyanocobaltate.
[0051] In the present invention, the water is preferably deionized water.
[0052] In the present invention, the molar ratio of the soluble nickel salt, the chelating agent and the hexacyanocobaltate is preferably (0.6-0.8): (0.6-0.9): (0.2-0.6), and more preferably (0.6-0.7): (0.7-0.8): (0.3-0.5).
[0053] In the present invention, the molar concentration of hexacyanocobaltate in the precursor solution is 5 to 15 mmol / L.
[0054] In the present invention, the mixing preferably includes:
[0055] first mixing a soluble nickel salt, a chelating agent and a portion of water to obtain a first mixed solution;
[0056] mixing the hexacyanocobaltate and the remaining water for a second time to obtain a hexacyanocobaltate solution;
[0057] The first mixed solution and the hexacyanocobaltate solution are mixed for a third time.
[0058] In the present invention, the molar concentration of the soluble nickel salt in the first mixed solution is preferably 30 to 40 mmol / L, more preferably 35 mmol / L.
[0059] In the present invention, the first mixing is preferably performed under stirring conditions. The present invention has no particular limitation on the stirring parameters, and parameters well known to those skilled in the art may be used.
[0060] In the present invention, the molar concentration of hexacyanocobaltate in the hexacyanocobaltate solution is preferably 10 to 30 mmol / L, more preferably 15 to 25 mmol / L, and even more preferably 18 to 20 mmol / L. The present invention does not particularly limit the second mixing process, and can be performed using a process well known to those skilled in the art.
[0061] In the present invention, the volume ratio of the first mixed solution to the hexacyanocobaltate solution is preferably 1:1. In the present invention, the third mixing is preferably performed under stirring; the stirring speed is preferably 120 rpm, and the stirring time is preferably 15 to 20 minutes, more preferably 16 to 19 minutes, and even more preferably 17 to 18 minutes. In a specific embodiment of the present invention, the stirring is preferably magnetic stirring.
[0062] In the present invention, the above-mentioned mixing process can make the solutions evenly mixed and the reaction more complete.
[0063] After obtaining the precursor solution, the present invention immerses the fiber substrate in the precursor and performs static aging to obtain the three-dimensional current collector.
[0064] Before the fiber base layer is impregnated, the present invention preferably further includes subjecting the fiber base layer to an acidification treatment. In the present invention, the acidification treatment process preferably includes the following steps: immersing the fiber base layer in a hydrochloric acid solution to perform a hydrothermal reaction.
[0065] In a specific embodiment of the present invention, the size of the fiber base layer is preferably 8 cm*10 cm.
[0066] In the present invention, the mass concentration of the hydrochloric acid solution is preferably 70%.
[0067] In the present invention, the hydrothermal reaction temperature is preferably 120-180°C, more preferably 130-170°C, and even more preferably 140-160°C; the reaction time is preferably 18-24 hours, more preferably 19-23 hours, and even more preferably 20-22 hours. In the present invention, the acidification treatment can improve the hydrophilicity of the fiber substrate, thereby achieving uniform nickel cobalt cyanide compounding.
[0068] After the hydrothermal reaction is completed, the present invention preferably further includes washing and drying the resulting fiber substrate. In the present invention, the washing is preferably performed sequentially with deionized water and then with alcohol; the deionized water wash is preferably performed three times, and the alcohol wash is preferably performed three times. The present invention does not particularly limit the drying process; it can be performed using a process well known to those skilled in the art.
[0069] The present invention has no special limitation on the impregnation process, and the process well known to those skilled in the art can be used. In a specific embodiment of the present invention, the area of the fiber base layer during impregnation is preferably 12 cm 2 .
[0070] In the present invention, the temperature of the static aging is preferably room temperature; the time is preferably 18 to 24 hours, more preferably 19 to 23 hours, and even more preferably 20 to 22 hours.
[0071] After the static aging is completed, the present invention also preferably includes washing and drying the obtained fiber base layer in sequence. In the present invention, the washing is preferably carried out in sequence by ultrapure water washing and alcohol washing; the number of ultrapure water washings is preferably 3 times, and the number of alcohol washings is preferably 3 times. In the present invention, the unreacted substances can be completely washed away by the above-mentioned washing, and there is no obvious residue on the surface. In the present invention, the drying temperature is preferably 50-60°C; the time is preferably >18h, and the morphology of the synthesized nickel cobalt cyanide is controlled by the reaction time.
[0072] The present invention also provides a lithium metal negative electrode, comprising a current collector and metallic lithium deposited on the current collector;
[0073] The current collector is the three-dimensional current collector described in the above technical solution or the three-dimensional current collector prepared by the preparation method described in the above technical solution.
[0074] In the present invention, the mass ratio of the current collector to metallic lithium is preferably 1:0.76-1.52, more preferably 1:0.9-1.4, and even more preferably 1:1.0-1.3.
[0075] In a specific embodiment of the present invention, the method for preparing the lithium metal negative electrode preferably includes the following steps:
[0076] A half-cell is assembled with the current collector as a working electrode, and metallic lithium is deposited on the current collector through a discharge reaction to obtain the lithium metal negative electrode.
[0077] In the present invention, the half-cell preferably includes a working electrode, a counter electrode, a separator and an electrolyte.
[0078] In the present invention, the working electrode is a current collector; the diameter of the current collector is preferably 12 mm.
[0079] In the present invention, the counter electrode is preferably lithium foil; the diameter of the lithium foil is preferably 13 mm, and the thickness is preferably 0.5 mm.
[0080] In the present invention, the diaphragm is preferably a polypropylene diaphragm, specifically a Celgard 2400 diaphragm.
[0081] In the present invention, the electrolyte preferably includes a lithium salt and an organic solvent.
[0082] In the present invention, the electrolyte preferably includes lithium bis(trifluoromethanesulfonyl imide) and lithium nitrate. In the present invention, the organic solvent preferably includes 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME). In the present invention, the volume ratio of 1,3-dioxolane and ethylene glycol dimethyl ether is preferably 1:1. In the present invention, the molar concentration of lithium bis(trifluoromethanesulfonyl imide) in the electrolyte is preferably 1 mol / L. In the present invention, the mass of the lithium nitrate is preferably 20% of the total mass of lithium bis(trifluoromethanesulfonyl imide and the organic solvent.
[0083] In the present invention, the half-cell is preferably assembled in an argon-filled glove box; the water content in the glove box is preferably <0.01 ppm, and the oxygen content is preferably <0.1 ppm. The present invention does not specifically limit the assembly process of the half-cell; procedures familiar to those skilled in the art can be used. In a specific embodiment of the present invention, the half-cell is a CR2016 button cell.
[0084] After the half-cell is assembled, the present invention preferably further includes allowing the half-cell to stand still; the standing time is preferably 8 hours.
[0085] In the present invention, the current density during the discharge reaction is preferably 0.5 mA / cm 2 ; The time is preferably 40h.
[0086] The present invention also provides the use of the three-dimensional current collector described in the above technical solution, the three-dimensional current collector prepared by the preparation method described in the above technical solution, or the lithium metal anode described in the above technical solution in a lithium-ion battery. The present invention does not particularly limit the specific implementation of the application, and can be carried out using processes familiar to those skilled in the art.
[0087] To further illustrate the present invention, a three-dimensional current collector, a preparation method and application thereof, a lithium metal negative electrode and its application provided by the present invention are described in detail below in conjunction with the accompanying drawings and examples, but they should not be understood as limiting the scope of protection of the present invention.
[0088] Example 1
[0089] The area is 6cm 2 The carbon cloth was placed in a hydrochloric acid solution with a mass concentration of 70%, and a hydrothermal reaction was carried out at 110° C. for 8 hours. The obtained carbon cloth was then washed with deionized water 3 times and alcohol 3 times in sequence, and dried to obtain an acidified carbon cloth.
[0090] Dissolve 0.6 mmol of nickel nitrate hexahydrate and 0.9 mmol of sodium citrate in 20 mL of deionized water under stirring to obtain a first mixed solution;
[0091] 0.4 mmol of potassium hexacyanocobaltate and 20 mL of deionized water were mixed to obtain a potassium hexacyanocobaltate solution; the first mixed solution obtained above and the potassium hexacyanocobaltate solution were stirred under magnetic stirring at a stirring speed of 120 r / min for 30 minutes to obtain a precursor solution;
[0092] The acidified carbon cloth obtained above was immersed in the precursor solution and aged at room temperature for 24 h. The carbon cloth was taken out and washed with ultrapure water 3 times and alcohol 3 times in sequence, and dried at 60°C overnight to obtain the three-dimensional current collector (wherein the loading amount of nickel-cobalt double metal cyanide was 1 mg cm -2 );
[0093] The three-dimensional current collector obtained above was cut into a disc with a diameter of 12 mm as a working electrode, a lithium foil with a diameter of 13 mm and a thickness of 0.5 mm was used as a counter electrode, polypropylene Celgard2400 was used as a separator, and a 1 mol / L lithium bistrifluoromethanesulfonyl imide solution was used as an electrolyte (the solvent was 1,3-dioxolane and ethylene glycol dimethyl ether in a volume ratio of 1:1, to which lithium bistrifluoromethanesulfonyl imide and LiNO3 were added at 20% of the total mass of the solvent) in an argon-filled glove box (wherein the moisture content was <0.01 ppm and the oxygen content was <0.1 ppm) to assemble into a CR2016 button cell;
[0094] After the button cell was left to stand for 8 hours, the current density was 0.5 mA / cm 2 The discharge reaction was carried out under the conditions of 40 hours to obtain the lithium metal negative electrode (wherein the mass ratio of the metal lithium to the current collector was 1:0.76).
[0095] Example 2
[0096] The area is 6cm 2 The carbon cloth was placed in a hydrochloric acid solution with a mass concentration of 70%, and a hydrothermal reaction was carried out at 110° C. for 8 hours. The obtained carbon cloth was then washed with deionized water 3 times and with alcohol 3 times in sequence, and then dried to obtain an acidified carbon cloth;
[0097] 1.2 mmol of nickel nitrate hexahydrate and 1.8 mmol of sodium citrate were dissolved in 20 mL of deionized water under stirring to obtain a first mixed solution;
[0098] 0.8 mmol of potassium hexacyanocobaltate and 20 mL of deionized water were mixed to obtain a potassium hexacyanocobaltate solution; the first mixed solution obtained above and the potassium hexacyanocobaltate solution were stirred under magnetic stirring at a stirring speed of 120 r / min for 30 minutes to obtain a precursor solution;
[0099] The acidified carbon cloth obtained above was immersed in the precursor solution and aged at room temperature for 24 h. The carbon cloth was taken out and washed with ultrapure water 3 times and alcohol 3 times in sequence, and dried at 60°C overnight to obtain the three-dimensional current collector (wherein the loading amount of nickel-cobalt double metal cyanide was 2 mg cm -2 );
[0100] The three-dimensional current collector obtained above was cut into a disc with a diameter of 12 mm as a working electrode, a lithium foil with a diameter of 13 mm and a thickness of 0.5 mm was used as a counter electrode, polypropylene Celgard2400 was used as a separator, and a 1 mol / L lithium bistrifluoromethanesulfonyl imide solution was used as an electrolyte (the solvent was 1,3-dioxolane and ethylene glycol dimethyl ether in a volume ratio of 1:1, to which lithium bistrifluoromethanesulfonyl imide and LiNO3 were added at 20% of the total mass of the solvent) in an argon-filled glove box (wherein the moisture content was <0.01 ppm and the oxygen content was <0.1 ppm) to assemble into a CR2016 button cell;
[0101] After the button cell was left to stand for 8 hours, the current density was 0.5 mA / cm 2 The discharge reaction was carried out under the conditions of 40 hours to obtain the lithium metal negative electrode (wherein the mass ratio of the metal lithium to the current collector was 1:1.52).
[0102] Comparative Example 1
[0103] The area is 6cm 2 The carbon cloth was placed in a hydrochloric acid solution with a mass concentration of 70%, and a hydrothermal reaction was carried out at 110° C. for 8 hours. The obtained carbon cloth was then washed with deionized water and alcohol for 6 times, and then dried to obtain an acidified carbon cloth;
[0104] Dissolve 0.6 mmol of nickel nitrate hexahydrate and 0.9 mmol of sodium citrate in 20 mL of deionized water under stirring to obtain a first mixed solution;
[0105] 0.4 mmol of potassium hexacyanocobaltate and 20 mL of deionized water were mixed to obtain a potassium hexacyanocobaltate solution; the first mixed solution obtained above and the potassium hexacyanocobaltate solution were stirred under magnetic stirring at a stirring speed of 120 r / min for 30 minutes to obtain a precursor solution;
[0106] The acidified carbon cloth obtained above was immersed in the precursor solution and aged at room temperature for 12 h. The carbon cloth was taken out and washed with ultrapure water and alcohol for 6 times, and dried at 60°C overnight to obtain the three-dimensional current collector (wherein the loading amount of nickel-cobalt double metal cyanide was 0.5 mg cm -2 ).
[0107] Comparative Example 2
[0108] The area is 6cm 2 The carbon cloth was placed in a hydrochloric acid solution with a mass concentration of 70%, and a hydrothermal reaction was carried out at 110° C. for 8 hours. The obtained carbon cloth was then washed with deionized water and alcohol for 6 times, and then dried to obtain an acidified carbon cloth;
[0109] Dissolve 0.6 mmol of nickel nitrate hexahydrate and 0.9 mmol of sodium citrate in 20 mL of deionized water under stirring to obtain a first mixed solution;
[0110] 0.4 mmol of potassium hexacyanocobaltate and 20 mL of deionized water were mixed to obtain a potassium hexacyanocobaltate solution; the first mixed solution obtained above and the potassium hexacyanocobaltate solution were stirred under magnetic stirring at a stirring speed of 120 r / min for 30 minutes to obtain a precursor solution;
[0111] The acidified carbon cloth obtained above was immersed in the precursor solution and aged at room temperature for 48 h. The carbon cloth was taken out and washed with ultrapure water and alcohol for 6 times, and dried at 60°C overnight to obtain the three-dimensional current collector (wherein the loading amount of nickel-cobalt double metal cyanide was 2 mg cm -2 ).
[0112] Performance Testing
[0113] Test Example 1
[0114] Scanning electron microscopy was performed on the blank carbon cloth and the three-dimensional current collectors obtained in Examples 1-2 and Comparative Examples 1-2. The SEM images obtained are as follows: Figures 1 to 5 As shown, Figure 1 For carbon cloth, Figure 2 For comparative example 1, Figure 3 For comparative example 2, Figure 4 For Example 1, Figure 5 For Example 2, Figure 1 and 2 It can be seen that only a small amount of nickel-cobalt double metal cyanide is loaded on the surface of the fiber; Figure 3 and 4 It can be seen that nickel-cobalt double metal cyanide is evenly coated on the fiber surface.
[0115] Test Example 2
[0116] The nickel-cobalt double metal cyanide loaded on the three-dimensional current collector in Example 1 was subjected to a transmission electron microscope scanning test, and the obtained TEM image is as follows: Figure 6 As shown, from Figure 6 It can be seen that the nickel-cobalt double metal cyanide is in a nanocubic structure with a side length of about 164 nm.
[0117] Test Example 3
[0118] The three-dimensional current collector obtained in Example 1 was subjected to X-ray diffraction test, and the obtained XRD pattern was as follows: Figure 7 As shown, from Figure 7 It can be seen that the present invention can successfully prepare nickel-cobalt double metal cyanide.
[0119] Test Example 4
[0120] The lithium metal negative electrode obtained in Example 1 was used as the working electrode, a lithium metal sheet with the same area as the lithium metal negative electrode was used as the counter electrode, polypropylene Celgard 2400 was used as the separator, and a 1 mol / L lithium bistrifluoromethanesulfonyl imide solution was used as the electrolyte (the solvent was 1,3-dioxolane and ethylene glycol dimethyl ether in a volume ratio of 1:1, to which lithium bistrifluoromethanesulfonyl imide and LiNO3 were added in an argon-filled glove box (wherein the moisture content was <0.01 ppm and the oxygen content was <0.1 ppm) to assemble a CR2016 button cell;
[0121] A carbon cloth without nickel-cobalt double metal cyanide loading was used as a current collector, and metallic lithium was deposited in the manner described in Example 1 to obtain a lithium metal negative electrode. The obtained lithium metal negative electrode was used as a control group for performance testing.
[0122] The cycle performance of the button battery was tested under the following conditions: the charge and discharge current density was 20 mA / cm 2 , the charge and discharge capacity is 10mAh / cm 2 ;
[0123] The test results are as follows Figure 8 As shown, from Figure 8 It can be seen that after 500 hours at a high current density, the hysteresis voltage of the lithium symmetrical battery assembled using the lithium negative electrode provided by the present invention remains at a low level of about 30.0 mV. Compared with the control group, it has a smaller polarization voltage and a longer and more stable cycle period.
[0124] Test Example 5
[0125] The lithium metal negative electrode obtained in Example 2 was used as the working electrode, a lithium metal sheet with the same area as the lithium metal negative electrode was used as the counter electrode, polypropylene Celgard 2400 was used as the separator, and a 1 mol / L lithium bistrifluoromethanesulfonyl imide solution was used as the electrolyte (the solvent was 1,3-dioxolane and ethylene glycol dimethyl ether in a volume ratio of 1:1, to which lithium bistrifluoromethanesulfonyl imide and LiNO3 were added in an amount of 20% of the total mass of the solvent) in an argon-filled glove box (wherein the moisture content was <0.01 ppm and the oxygen content was <0.1 ppm) to form a CR2016 button cell;
[0126] A carbon cloth without nickel-cobalt double metal cyanide loading was used as a current collector, and metallic lithium was deposited in the manner described in Example 2 to obtain a lithium metal negative electrode. The obtained lithium metal negative electrode was used as a control group for performance testing.
[0127] The cycle performance of the button battery was tested under the following conditions: the charge and discharge current density was 20 mA / cm 2 , the charge and discharge capacity is 10mAh / cm 2;
[0128] The test results are as follows Figure 9 As shown, from Figure 9 It can be seen that after 500 hours at a high current density, the hysteresis voltage of the lithium symmetrical battery assembled using the lithium negative electrode provided by the present invention remains at a low level of about 30.0 mV. Compared with the control group, it has a smaller polarization voltage and a longer and more stable cycle period.
[0129] Test Example 6
[0130] The performance test was carried out according to the method in Test Example 1, where the test conditions were: the charge and discharge current density was 40 mA / cm 2 , the charge and discharge capacity is 20mAh / cm 2 ;
[0131] The test results are as follows Figure 10 As shown, from Figure 10 It can be seen that after 5600 hours at an ultra-high current density, the hysteresis voltage of the lithium symmetrical battery assembled using the lithium negative electrode provided by the present invention remains at a low level of about 23.0 mV. Compared with the control group, it has a smaller polarization voltage and a longer and more stable cycle period.
[0132] Although the above embodiment provides a detailed description of the present invention, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A three-dimensional current collector, It is characterized in that It includes a fiber base and nickel-cobalt double metal cyanide loaded in the fiber base; The fiber base layer has a three-dimensional porous structure; The morphology of the nickel-cobalt double metal cyanide is a cubic structure.
2. The three-dimensional current collector according to claim 1, It is characterized in that The loading amount of the nickel-cobalt double metal cyanide is 0.5 to 2 mg·cm -2 .
3. A method for preparing a three-dimensional current collector according to any one of claims 1 to 2, It is characterized in that The following steps are involved: mixing a soluble nickel salt, a chelating agent, hexacyanocobaltate and water to obtain a precursor solution; The fiber substrate is immersed in the precursor solution and subjected to static aging to obtain the three-dimensional current collector.
4. The preparation method according to claim 3, It is characterized in that The soluble nickel salt includes one or more of nickel nitrate, nickel acetate and sulfate; The chelating agent includes one or more of citrate, phosphate and aminocarboxylic acid chelating agents.
5. The preparation method according to claim 3 or 4, It is characterized in that The molar ratio of the soluble nickel salt, the chelating agent and the hexacyanocobaltate is (0.6-0.8): (0.6-0.9): (0.2-0.6); The molar concentration of hexacyanocobaltate in the precursor solution is 5 to 15 mmol / L.
6. The preparation method according to claim 3, It is characterized in that The mixing includes: The soluble nickel salt, the chelating agent and part of the water are first mixed to obtain a first mixed solution; mixing the hexacyanocobaltate and the remaining water for a second time to obtain a hexacyanocobaltate solution; The first mixed solution and the hexacyanocobaltate solution are mixed for the third time.
7. The preparation method according to claim 3, It is characterized in that The temperature of the static aging is room temperature, and the time is 18 to 24 hours.
8. A lithium metal negative electrode comprising a current collector and metallic lithium deposited on the current collector, It is characterized in that The current collector is the three-dimensional current collector according to any one of claims 1 to 2 or the three-dimensional current collector prepared by the preparation method according to any one of claims 3 to 7.
9. The preparation method according to claim 8, It is characterized in that The mass ratio of the current collector to metallic lithium is 1:0.76-1.
52.
10. Use of the three-dimensional current collector according to any one of claims 1 to 2, the three-dimensional current collector prepared by the preparation method according to any one of claims 3 to 7, or the lithium metal negative electrode according to any one of claims 8 to 9 in a lithium ion battery.
Citation Information
Patent Citations
Preparation of bimetallic sulfide with conductive carbon cloth as substrate and application thereof in negative pole of lithium-ion battery
CN110299510A
Method of producing conductive particle for negative electrode and method of producing nickel metal hydride battery
JP2019117778A
KR20220115754A