Thermoplastic resin composition and molded article made therefrom

Through the combination of polycarbonate resin, polyester resin, glass fiber, talc and phosphazene flame retardants, the degradation problems of polycarbonate resin in terms of dimensional stability, flame retardancy, impact resistance and color are solved, achieving Balanced properties of thermoplastic resin compositions suitable for materials used in electrical/electronic products.

CN115989278BActive Publication Date: 2024-10-08LOTTE CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180052229.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-31
Filing Date
2021-08-03
Publication Date
2024-10-08
Estimated Expiration
2041-08-03

AI Technical Summary

Technical Problem

Existing polycarbonate resins have degradation problems in terms of dimensional stability, flame retardancy, impact resistance and color, making it difficult to achieve a metal-level performance balance.

Method used

Using about 100 parts by weight of polycarbonate resin, about 0.7 to 12 parts by weight of polyester resin, about 35 to 85 parts by weight of glass fiber, about 5 to 40 parts by weight of talc and about 4 to 28 parts by weight of phosphazene barrier A combination of fuel agent, glass fiber and talc are present in a weight ratio of 1.5:1 to 6:1, and a thermoplastic resin composition is prepared through a twin-screw extruder.

Benefits of technology

Achieved good properties of the thermoplastic resin composition in terms of dimensional stability, flame retardancy, impact resistance and color, with a linear expansion coefficient of 35 μm/m·℃ to 50 μm/m·℃, a flame retardancy of V-0, and a notch The Izod impact strength is 7.5kgf·cm/cm to 20kgf·cm/cm, and the yellowness index is 2 to 10.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004092366520000061
    Figure BDA0004092366520000061
  • Figure BDA0004092366520000091
    Figure BDA0004092366520000091
  • Figure BDA0004092366520000101
    Figure BDA0004092366520000101
Patent Text Reader

Abstract

The thermoplastic resin composition of the present invention includes: polycarbonate resin; polyester resin; rectangular cross-section glass fiber having a cross-sectional aspect ratio of about 1.5 to about 10, a cross-sectional minor diameter of about 2 to about 10 μm, and a pre-processing length of about 1 to about 30 mm; talc having an average particle size (D50) of about 7 to about 30 μm; and a phosphazene flame retardant, wherein the weight ratio of the glass fiber to the talc is about 1.5:1 to about 6:1. The thermoplastic resin composition has excellent dimensional stability, flame retardancy, impact resistance, color, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermoplastic resin composition and a molded article made therefrom. More specifically, the present invention relates to a thermoplastic resin composition showing good characteristics in terms of dimensional stability, flame retardancy, impact resistance and color, and a molded article made therefrom. Background Art

[0002] As an engineering plastic, polycarbonate resin has excellent properties in terms of impact resistance, heat resistance, dimensional stability, weather resistance, flame retardancy, electrical properties, and transparency, and is usefully applied to housings of electrical / electronic products and interior / exterior materials of office equipment, etc. In addition, various fillers are used to improve various properties of polycarbonate resin.

[0003] However, fillers used to improve the dimensional stability of polycarbonate resins, such as glass fiber, talc, and wollastonite, have different physical properties depending on the type of filler, and may cause difficulty in achieving color due to an increase in yellowness index, and may cause difficulty in achieving dimensional stability at a metal level due to deterioration of properties when added in a certain amount or more.

[0004] Therefore, there is a need to develop a thermoplastic resin composition that can achieve dimensional stability at a metal level and exhibit good characteristics in terms of flame retardancy, impact resistance, color, and the like.

[0005] The background art of the present invention is disclosed in Korean Patent Laid-Open Publication No. 10-2011-0059886 and the like. Summary of the invention

[0006] Technical issues

[0007] An object of the present invention is to provide a thermoplastic resin composition showing good characteristics in terms of dimensional stability, flame retardancy, impact resistance and color.

[0008] Another object of the present invention is to provide a molded article produced from the thermoplastic resin composition.

[0009] The above objects and other objects of the present invention can be achieved by the present invention described below.

[0010] Technical Solution

[0011] 1. One aspect of the present invention relates to a thermoplastic resin composition. The thermoplastic resin composition includes: about 100 parts by weight of a polycarbonate resin; about 0.7 parts by weight to about 12 parts by weight of a polyester resin; about 35 parts by weight to about 85 parts by weight of glass fiber, the glass fiber having a rectangular cross-section, a cross-sectional aspect ratio (long side length / short side length in the cross-section) of about 1.5 to about 10, a short side length of about 2 μm to about 10 μm, and a pre-processing length of about 1 mm to about 30 mm; about 5 parts by weight to about 40 parts by weight of talc, the talc having an average particle size (D50) of about 7 μm to about 30 μm; and about 4 parts by weight to about 28 parts by weight of a phosphazene flame retardant, wherein the glass fiber and the talc are present in a weight ratio of about 1.5:1 to about 6:1.

[0012] 2. In embodiment 1, the polyester resin may include at least one of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polytrimethylene terephthalate, and polycyclohexylene terephthalate.

[0013] 3. In embodiment 1 or 2, the polyester resin may include at least one of polyethylene terephthalate and polybutylene terephthalate.

[0014] 4. In embodiments 1 to 3, the polyester resin and the glass fiber may be present in a weight ratio of about 1:5 to about 1:50.

[0015] 5. In embodiments 1 to 4, when an injection molded sample having a size of 127 mm×12.7 mm×3.2 mm is heated from 0°C to 60°C at 5°C / min in accordance with ASTM D696, the coefficient of linear expansion of the thermoplastic resin composition in a direction transverse to the resin flow may be about 35 μm / m·°C to about 50 μm / m·°C.

[0016] 6. In embodiments 1 to 5, the flame retardancy of the thermoplastic resin composition may be V-0 when measured on a 0.8 mm thick sample by the UL-94 vertical test method.

[0017] 7. In embodiments 1 to 6, the thermoplastic resin composition may have a notched Izod impact strength of about 7.5 kgf·cm / cm to about 20 kgf·cm / cm when measured on a 1 / 8" thick notched Izod specimen according to ASTM D256.

[0018] 8. In embodiments 1 to 7, the yellowness index (YI) of the thermoplastic resin composition may be about 2 to about 10 according to ASTM D1925.

[0019] 9. Another aspect of the present invention relates to a molded article. The molded article is made of the thermoplastic resin composition according to any one of Embodiments 1 to 8.

[0020] 10. In embodiment 9, the molded article may have a longitudinal length of about 100 cm to about 300 cm, a transverse length of about 50 cm to about 150 cm, and a thickness of about 0.1 mm to about 10 mm, and may be manufactured by extrusion and injection molding.

[0021] Beneficial Effects

[0022] The present invention provides a thermoplastic resin composition having excellent characteristics in terms of dimensional stability, flame retardancy, impact resistance, color, etc., and a molded article produced therefrom. DETAILED DESCRIPTION

[0023] Hereinafter, embodiments of the present invention will be described in detail.

[0024] The thermoplastic resin composition according to the present invention includes: (A) a polycarbonate resin; (B) a polyester resin; (C) glass fiber; (D) talc; and (E) a phosphazene flame retardant.

[0025] As used herein, in order to express a specific numerical range, the expression “a to b” means “≥a and ≤b”.

[0026] (A) Polycarbonate resin

[0027] The polycarbonate resin according to one embodiment of the present invention may include any polycarbonate resin used in a typical thermoplastic resin composition. For example, the polycarbonate resin may be an aromatic polycarbonate resin prepared by reacting a biphenol (aromatic diol compound) with a precursor (such as phosgene, halogen formate or carbonate diester).

[0028] In some embodiments, the biphenol may include, for example, 4,4'-diphenol, 2,2-bis(4-hydroxyphenyl)propane, 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2-bis(3-chloro-4-hydroxyphenyl)propane, and 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, but is not limited thereto. For example, the biphenol may be 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, or 1,1-bis(4-hydroxyphenyl)cyclohexane, specifically 2,2-bis(4-hydroxyphenyl)propane, which is also known as bisphenol A.

[0029] In some embodiments, the polycarbonate resin may be a branched polycarbonate resin. For example, the polycarbonate resin may be a polycarbonate resin prepared by adding a trifunctional or higher functional polyfunctional compound, specifically a trivalent or higher valent phenol group-containing compound, in an amount of about 0.05 mol% to about 2 mol% based on the total moles of biphenol used in the polymerization.

[0030] In some embodiments, the polycarbonate resin may be a homopolycarbonate resin, a copolycarbonate resin, or a blend thereof. In addition, the polycarbonate resin may be partially or completely replaced by an aromatic polyester-carbonate resin obtained by polymerization in the presence of an ester precursor (eg, a difunctional carboxylic acid).

[0031] In some embodiments, the polycarbonate resin may have a weight average molecular weight (Mw) of about 10,000 g / mol to about 200,000 g / mol, for example, about 15,000 g / mol to about 80,000 g / mol, when measured by gel permeation chromatography (GPC). Within this range, the thermoplastic resin composition may have good fluidity (processing properties).

[0032] (B) Polyester resin

[0033] According to the present invention, the polyester resin is used to achieve the dimensional stability of the metal level of the thermoplastic resin composition together with the polycarbonate resin, the glass fiber and the talc, etc., without deteriorating other properties such as impact resistance, flame retardancy and color, etc., and can be selected from any polyester resin used in a typical thermoplastic resin composition. For example, the polyester resin can be obtained by polycondensation of a dicarboxylic acid component and a diol component, wherein the dicarboxylic acid component may include: aromatic dicarboxylic acids such as terephthalic acid (TPA), isophthalic acid (IPA), 1,2-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid and 2,7-naphthalene dicarboxylic acid, etc.; and aromatic dicarboxylic acid esters such as dimethyl terephthalate (DMT), isophthalic acid (IPA), 1,2-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid and 2,7-naphthalene dicarboxylic acid, etc.; The present invention relates to a novel polyol having a plurality of polyols, for example, polyols of the present invention, wherein the polyols include dimethyl 1,2-naphthalene dicarboxylate, dimethyl 1,5-naphthalene dicarboxylate, dimethyl 1,7-naphthalene dicarboxylate, dimethyl 1,8-naphthalene dicarboxylate, dimethyl 2,3-naphthalene dicarboxylate, dimethyl 2,6-naphthalene dicarboxylate and dimethyl 2,7-naphthalene dicarboxylate, and the diol component may include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2,2-dimethyl-1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol and cycloolefin diol.

[0034] In some embodiments, the polyester resin may include at least one of polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polytrimethylene terephthalate (PTT), and polycyclohexyl terephthalate. For example, the polyester resin may be polyethylene terephthalate, polybutylene terephthalate, or a combination thereof.

[0035] In some embodiments, the polyester resin may have an intrinsic viscosity of about 0.6 dl / g to about 1.5 dl / g, for example, about 0.7 dl / g to about 1.3 dl / g, when measured in an o-chlorophenol solution (concentration: 0.5 g / dl) using an Ubbelohde viscometer (capillary viscometer) at 25° C. Within this range, the thermoplastic resin composition may exhibit good processability, dimensional stability, and the like.

[0036] In some embodiments, the polyester resin may be present in an amount of about 0.7 parts by weight to about 12 parts by weight, for example, about 1 part by weight to about 10 parts by weight, relative to about 100 parts by weight of the polycarbonate resin. If the content of the polyester resin is less than about 0.7 parts by weight relative to about 100 parts by weight of the polycarbonate resin, the thermoplastic resin composition may suffer from deterioration in dimensional stability, etc., and if the content of the polyester resin exceeds about 12 parts by weight, the thermoplastic resin composition may suffer from deterioration in flame retardancy and impact resistance, etc.

[0037] (C) Fiberglass

[0038] According to the present invention, glass fiber is used together with polycarbonate resin, polyester resin, talc, etc. to achieve dimensional stability at a metal level of a thermoplastic resin composition without deteriorating other characteristics such as flame retardancy, impact resistance, color, and the like.

[0039] In some embodiments, the glass fiber may have a rectangular cross section. When measured by a scanning electron microscope (manufacturer: JEOL, model: JSM-6390A), the glass fiber with a rectangular cross section may have a cross-sectional aspect ratio (long side length / short side length in the cross section) of about 1.5 to about 10, for example, about 2 to about 8, about 2 μm to about 10 μm, for example, about 4 μm to about 8 μm of short side length, and about 1 mm to about 30 mm, for example, about 2 mm to about 16 mm of pre-processing length. Within this range, the thermoplastic resin composition can have good characteristics in terms of dimensional stability, rigidity and processability.

[0040] In some embodiments, the glass fibers may be surface treated with a typical surface treatment agent.

[0041] In some embodiments, the glass fiber may be present in an amount of about 35 parts by weight to about 85 parts by weight, for example, about 40 parts by weight to about 80 parts by weight, relative to about 100 parts by weight of the polycarbonate resin. If the content of the glass fiber is less than about 35 parts by weight relative to about 100 parts by weight of the polycarbonate resin, the thermoplastic resin composition may suffer from deterioration in dimensional stability, etc., and if the content of the glass fiber exceeds about 85 parts by weight, the thermoplastic resin composition may suffer from deterioration in impact resistance and flame retardancy, etc.

[0042] In some embodiments, the polyester resin (B) and the glass fiber (C) may be present in a weight ratio (B:C) of about 1:5 to about 1:50, for example, about 1:8 to about 1:40. Within this range, the thermoplastic resin composition may exhibit good properties in terms of dimensional stability and impact resistance.

[0043] (D) Talc

[0044] According to the present invention, talc is used to achieve dimensional stability at a metal level of a thermoplastic resin composition together with a polycarbonate resin, a polyester resin, a glass fiber, and the like without deteriorating other characteristics including flame retardancy, impact resistance, color, and the like.

[0045] In some embodiments, the talc may be a plate-like filler, and when measured by a laser particle analyzer (manufacturer: Beckman Coulter, model: LS 13 320), the talc may have an average particle size (D50) of about 7 μm to about 30 μm, for example, about 10 μm to about 20 μm. If the average particle size of the talc exceeds this range, the thermoplastic resin composition may suffer from deterioration in dimensional stability, rigidity, processability, etc.

[0046] In some embodiments, the talc may be present in an amount of about 5 parts by weight to about 40 parts by weight, for example, about 10 parts by weight to about 30 parts by weight, relative to about 100 parts by weight of the polycarbonate resin. If the content of the talc is less than about 5 parts by weight relative to about 100 parts by weight of the polycarbonate resin, the thermoplastic resin composition may suffer from deterioration in dimensional stability, etc., and if the content of the talc exceeds about 40 parts by weight, the thermoplastic resin composition may suffer from deterioration in impact resistance and flame retardancy, etc.

[0047] In some embodiments, the glass fiber and the talc may be present in a weight ratio (C:D) of about 1.5: 1 to about 6: 1, for example, about 2: 1 to about 6: 1. If the weight ratio of the glass fiber to the talc is less than about 1.5: 1, the thermoplastic resin composition may suffer from deterioration in impact resistance, etc., and if the weight ratio of the glass fiber to the talc exceeds about 6: 1, the thermoplastic resin composition may suffer from deterioration in dimensional stability, etc.

[0048] (E) Phosphazene flame retardant

[0049] The phosphazene flame retardant according to one embodiment of the present invention is used to improve flame retardancy, impact resistance, etc. of a thermoplastic resin composition and may include a phosphazene compound used for a typical flame retardant thermoplastic resin composition.

[0050] In some embodiments, the phosphazene flame retardant may include a phosphazene compound represented by Formula 1.

[0051] [Formula 1]

[0052]

[0053] wherein R1, R2, R3, R4, R5 and R6 are each independently a hydrogen atom, a halogen atom, a substituted or unsubstituted C1 to C 20 alkyl, substituted or unsubstituted C2 to C7 alkenyl, substituted or unsubstituted C3 to C 20 Cycloalkyl, substituted or unsubstituted C2 to C 20 Heterocycloalkyl, C1 to C 20 Alkoxy, C6 to C 20 Aryl or aryloxy, C5 to C 20 Heteroaryl, substituted or unsubstituted C3 to C 20 Alkoxycarbonylalkyl, substituted or unsubstituted C2 to C 10 carbonylalkyl, amino or hydroxy.

[0054] Here, "substituted" means that a hydrogen atom is replaced by a substituent, for example, C1 to C 10 Alkyl, halogen, nitro, cyano, hydroxyl, amino, C6 to C 10 Aryl, C3 to C 10 Cycloalkyl, C3 to C 10 Heterocycloalkyl, C4 to C 10 Heteroaryl and combinations thereof.

[0055] In addition, "alkyl", "alkoxy" and other substituents containing an "alkyl" portion include straight or branched structures, and "alkenyl" includes a straight or branched structure having 2 to 8 carbon atoms and containing at least one double bond. In addition, "cycloalkyl" includes a saturated monocyclic structure or a saturated bicyclic structure having 3 to 20 carbon atoms. In addition, "aryl" is an organic radical derived from an aromatic hydrocarbon by removing a hydrogen atom from the aromatic hydrocarbon and includes a monocyclic system or a condensed ring system containing appropriately 4 to 7, preferably 5 or 6 atoms in each ring. Specifically, "aryl" may include phenyl, naphthyl, biphenyl and tolyl, etc.

[0056] Here, "heterocycloalkyl" means a cycloalkyl group containing 1 to 3 heteroatoms selected from N, O and S as saturated cyclic hydrocarbon backbone atoms, wherein the remaining saturated monocyclic or bicyclic ring backbone atoms are carbon atoms, and may include pyrrolidinyl, azetidinyl, pyrazolidinyl, oxazolidinyl, piperidinyl, piperazinyl, morpholinyl, thiomorpholinyl, thiazolidinyl, hydantoinyl, valerolactamyl, oxylanyl, oxetanyl, dioxolanyl, dioxanyl, oxathiolanyl, oxathiolanyl, dithianyl, dihydrofuranyl, tetrahydrofuranyl, dihydropyranyl, tetrahydropyranyl, tetrahydropyridinyl, tetrahydropyrimidinyl, tetrahydrothiophenyl, tetrahydrothiopyranyl, diazepanyl and azepanyl, etc.

[0057] In addition, "heteroaryl" means an aryl group containing 1 to 3 heteroatoms selected from N, O and S as aromatic ring backbone atoms, wherein the remaining ring backbone atoms are carbon atoms. Heteroaryl groups may include divalent aryl groups in which the heteroatoms in the ring are oxidized or quaternized to form, for example, N-oxides or quaternary salts. Specifically, heteroaryl groups may include furanyl, thienyl, pyrrolyl, pyranyl, imidazolyl, pyrazolyl, thiazolyl, thiadiazolyl, isothiazolyl, isoxazolyl, oxazolyl, oxadiazolyl, triazinyl, tetrazinyl, triazolyl, tetrazolyl, furazanyl, pyridyl, pyrazinyl, pyrimidinyl and pyridazinyl, etc.

[0058] In some embodiments, the phosphazene flame retardant may be present in an amount of about 4 parts by weight to about 28 parts by weight, for example, about 5 parts by weight to about 25 parts by weight, relative to about 100 parts by weight of the polycarbonate resin. If the content of the phosphazene flame retardant is less than about 4 parts by weight relative to about 100 parts by weight of the polycarbonate resin, the thermoplastic resin composition may suffer from deterioration in flame retardancy, fluidity, etc., and if the content of the phosphazene flame retardant exceeds about 28 parts by weight, the thermoplastic resin composition may suffer from deterioration in impact resistance, dimensional stability, etc.

[0059] In some embodiments, the thermoplastic resin composition may further include an additive for a typical thermoplastic resin composition. Examples of additives may include antioxidants, anti-dripping agents, lubricants, mold release agents, nucleating agents, antistatic agents, stabilizers, pigments, dyes, and mixtures thereof, but are not limited thereto. The additive may be present in an amount of about 0.001 parts by weight to about 40 parts by weight, for example, about 0.1 parts by weight to about 10 parts by weight, relative to about 100 parts by weight of the polycarbonate resin.

[0060] In some embodiments, the thermoplastic resin composition may be prepared in the form of pellets by mixing the aforementioned components and then melt-extruding using a typical twin-screw extruder at about 200°C to about 280°C, for example, about 220°C to about 270°C.

[0061] In some embodiments, the thermoplastic resin composition may have a linear expansion coefficient of about 35 μm / m·°C to about 50 μm / m·°C, for example, about 40 μm / m·°C to about 49 μm / m·°C, in a direction transverse to resin flow, when measured on an injection molded sample having a size of 127 mm×12.7 mm×3.2 mm while being heated from 0°C to 60°C at 5°C / min using a thermomechanical analyzer in accordance with ASTM D696.

[0062] In some embodiments, the thermoplastic resin composition may have a flame retardancy of V-0 when measured by a UL-94 vertical test method on a 0.8 mm thick injection molded sample.

[0063] In some embodiments, the thermoplastic resin composition may have a notched Izod impact strength of about 7.5 kgf·cm / cm to about 20 kgf·cm / cm, for example, about 8 kgf·cm / cm to about 15 kgf·cm / cm, when measured on a 1 / 8" thick sample according to ASTM D256.

[0064] In some embodiments, the thermoplastic resin composition may have a yellowness index (YI) of about 2 to about 10, for example, about 3 to about 8, when measured according to ASTM D1925.

[0065] The molded article according to the present invention is manufactured by the thermoplastic resin composition as stated above. The thermoplastic resin composition can be prepared in the form of pellets. The prepared pellets can be produced as various molded articles (articles) by various molding methods, such as injection molding, extrusion molding, vacuum molding and casting. These molding methods are well known to those skilled in the art. The molded article has good properties in terms of dimensional stability, flame retardancy, impact resistance, color and the balance therebetween, and can therefore be advantageously used for internal / external materials and thin sheets of electrical / electronic products, etc.

[0066] In some embodiments, when measured on an injection molded sample having a size of 127 mm×12.7 mm×3.2 mm while being heated from 0°C to 60°C at 5°C / min in accordance with ASTM D696, the linear expansion coefficient of the molded article in the transverse direction of the resin flow may be about 35 μm / m·°C to about 50 μm / m·°C; the flame retardancy of the molded article may be V-0 when measured on a 0.8 mm thick injection molded sample by the UL-94 vertical test method; the notched Izod impact strength of the molded article may be about 7.5 kgf·cm / cm to about 20 kgf·cm / cm when measured on a 1 / 8” thick sample in accordance with ASTM D256, and the The molded article has a yellowness index (YI) of about 2 to about 10 when measured by D1925, and the molded article can be advantageously used for large extrusion and injection molded products (for interior / exterior materials of electrical / electronic products) having a longitudinal length of about 100 cm to about 300 cm, a transverse length of about 50 cm to about 150 cm, and a thickness of about 0.1 mm to about 10 mm.

[0067] Implementation

[0068] Next, the present invention will be described in more detail with reference to some examples. It should be understood that these examples are provided only for illustration and are by no means construed as limiting the present invention.

[0069] Example

[0070] The details of the components used in Examples and Comparative Examples are as follows.

[0071] (A) Polycarbonate resin

[0072] A bisphenol A polycarbonate resin having a weight average molecular weight (Mw) of 25,000 g / mol was used.

[0073] (B) Polyester resin

[0074] Polyethylene terephthalate (PET, manufacturer: Lotte Chemical Co., Ltd., intrinsic viscosity: 0.765 dl / g) was used.

[0075] (C) Fiberglass

[0076] (C1) Glass fiber having a rectangular cross section, a cross-sectional aspect ratio (long side length / short side length in cross section) of 4, a short side length of 7 μm, and a pre-processed length of 3 mm was used (manufacturer: Nittobo Co., Ltd., product name: CSG 3PA-832).

[0077] (C2) A glass fiber having a circular cross section, a cross-sectional diameter of 13 μm, and a pre-processed length of 3 mm (manufacturer: KCC, product name: CS321-EC10-3) was used.

[0078] (D) Inorganic fillers

[0079] (D1) Talc (manufacturer: KOCH, product name: KCP-04) having an average particle size (D50) of 12 μm was used.

[0080] (D2) Talc (manufacturer: KOCH, product name: KCM-6300) having an average particle size (D50) of 6 μm was used.

[0081] (D3) Mica (manufacturer: IMERYS Co., Ltd., product name: 60-S) having an average particle size (D50) of 400 μm was used.

[0082] (E) Phosphorus flame retardant

[0083] (E1) A phosphazene compound (manufacturer: Fushimi Pharmaceutical Co., Ltd., product name: Rabitle FP-110) was used.

[0084] (E2) Bisphenol A diphosphate (manufacturer: Yoke Chemical Co., Ltd., product name: YOKEBDP) was used.

[0085] Examples 1 to 9 and Comparative Examples 1 to 14

[0086] The above components were mixed in the amounts listed in Tables 1 to 3 and extruded at 260° C. to prepare a thermoplastic resin composition in the form of pellets. A twin-screw extruder (L / D=36, Φ: 45 mm) was used for extrusion and the prepared pellets were dried at 80° C. for 4 hours or more and injection molded in a 6-ounce injection molding machine (molding temperature: 260° C., mold temperature: 60° C.) to prepare a sample. The following properties of the prepared samples were evaluated by the following methods, and the results are shown in Tables 1 to 3.

[0087] Characteristic measurement

[0088] (1) Dimensional stability: In accordance with ASTM D696, the linear expansion coefficient (unit: μm / m·°C) of an injection molded sample having a size of 127 mm×12.7 mm×3.2 mm was measured in a direction transverse to the resin flow using a thermomechanical analyzer while the sample was heated from 0°C to 60°C at 5°C / min.

[0089] (2) Flame retardancy: Flame retardancy was measured on 0.8 mm thick injection molded specimens by the UL-94 vertical test method.

[0090] (3) Impact resistance: Notched Izod impact strength (kgf·cm / cm) was measured on 1 / 8" thick samples according to ASTM D256.

[0091] (4) Color: The yellowness index (YI) was measured according to ASTM D1925.

[0092] Table 1

[0093]

[0094]

[0095] Table 2

[0096]

[0097] Table 3

[0098]

[0099]

[0100] As can be seen from the results, the thermoplastic resin composition according to the present invention has excellent characteristics in terms of dimensional stability, flame retardancy, impact resistance, color, and the like.

[0101] On the contrary, it can be seen that the thermoplastic resin composition prepared using an insufficient amount of polyester resin (Comparative Example 1) suffers from deterioration in dimensional stability, etc.; the thermoplastic resin composition prepared using an excessive amount of polyester resin (Comparative Example 2) suffers from deterioration in flame retardancy and impact resistance, etc.; the thermoplastic resin composition prepared using an insufficient amount of glass fiber (Comparative Example 3) suffers from deterioration in dimensional stability, etc.; and the thermoplastic resin composition prepared using an excessive amount of glass fiber (Comparative Example 4) suffers from deterioration in impact resistance, etc.; and the thermoplastic resin composition prepared using glass fiber (C2) instead of the glass fiber of the present invention (Comparative Example 5) suffers from deterioration in flame retardancy and bending properties, etc. In addition, it can be seen that the thermoplastic resin composition prepared using insufficient talc (Comparative Example 6) suffers from deterioration in dimensional stability and flame retardancy, etc.; the thermoplastic resin composition prepared using excessive talc (Comparative Example 7) suffers from deterioration in impact resistance, etc.; the thermoplastic resin composition prepared using talc (D2) instead of the talc of the present invention (Comparative Example 8) suffers from deterioration in dimensional stability, etc.; and the thermoplastic resin composition prepared using mica (D3) (Comparative Example 9) suffers from difficulty in achieving color, etc. In addition, it can be seen that the thermoplastic resin composition prepared using insufficient phosphazene flame retardant (Comparative Example 10) suffers from deterioration in flame retardancy, etc.; the thermoplastic resin composition prepared using excessive phosphazene flame retardant (Comparative Example 11) suffers from deterioration in impact resistance and dimensional stability, etc.; and the thermoplastic resin composition prepared using BSP (E2) instead of the phosphazene flame retardant according to the present invention (Comparative Example 12) suffers from deterioration in flame retardancy, etc. In addition, it can be seen that the thermoplastic resin composition prepared using an insufficient weight ratio (1:1) of glass fiber and talc (Comparative Example 13) suffers from deterioration in impact resistance, etc.; and the thermoplastic resin composition prepared using an excessively large weight ratio (7:1) of glass fiber and talc (Comparative Example 14) suffers from deterioration in dimensional stability, etc.

[0102] Although some exemplary embodiments have been described herein, it will be appreciated by those skilled in the art that these embodiments are given only by way of illustration, and that various modifications, variations and changes may be made without departing from the spirit and scope of the present invention. Therefore, the embodiments should not be interpreted as limiting the technical spirit of the present invention, but rather as explaining the technical spirit of the present invention. The scope of the present invention should be interpreted according to the appended claims as covering all modifications or variations derived from the appended claims and their equivalents.

Claims

1. A thermoplastic resin composition, include: 100 parts by weight of polycarbonate resin; 0.7 to 12 parts by weight of a polyester resin; 35 to 85 parts by weight of glass fiber having a rectangular cross section, a cross-sectional aspect ratio of 1.5 to 10, a short side length of 2 to 10 μm, and a pre-processed length of 1 to 30 mm; 5 to 40 parts by weight of talc having an average particle size D50 of 7 to 30 μm; and 4 to 28 parts by weight of a phosphazene flame retardant, wherein the cross-sectional aspect ratio refers to the long side length / short side length in the cross section, wherein the glass fiber and the talc are present in a weight ratio of 1.5:1 to 6:1, The polyester resin includes at least one of polyethylene terephthalate and polybutylene terephthalate. 2 . The thermoplastic resin composition according to claim 1 , wherein the polyester resin and the glass fiber are present in a weight ratio of 1:5 to 1:

50.

3. The thermoplastic resin composition according to claim 1 or 2, wherein the coefficient of linear expansion of the thermoplastic resin composition in a direction transverse to resin flow is 35 μm / m·°C to 50 μm / m·°C when measured on an injection molded sample having a size of 127 mm×12.7 mm×3.2 mm while the sample is heated from 0°C to 60°C at 5°C / min in accordance with ASTM D696. 4 . The thermoplastic resin composition according to claim 1 , wherein the flame retardancy of the thermoplastic resin composition is V-0 when measured on a 0.8 mm thick sample by a UL-94 vertical test method.

5. The thermoplastic resin composition according to claim 1 or 2, wherein the notched Izod impact strength of the thermoplastic resin composition is 7.5 to 20 kgf·cm / cm when measured on a 1 / 8" thick notched Izod specimen according to ASTM D256. 6 . The thermoplastic resin composition according to claim 1 , wherein the thermoplastic resin composition has a yellowness index YI of 2 to 10 according to ASTM D1925. 7 . A molded article produced from the thermoplastic resin composition according to claim 1 . 8 . The molded article according to claim 7 , wherein the molded article has a longitudinal length of 100 cm to 300 cm, a lateral length of 50 cm to 150 cm, and a thickness of 0.1 mm to 10 mm.

Citation Information

Patent Citations

  • Stress cracking-resistant and low-warpage two-component molded parts comprising talcum

    KR1020110059886A

  • Composition of phosphagen thermoplastic resin havingsuperior flame retardant

    KR1020010109044A

  • Flame retardant polycarbonate compositions, methods of manufacture thereof and articles comprising the same

    US20130317144A1

  • Thermoplastic Resin Composition and Article Comprising the Same

    US20150344670A1

  • Glass-fiber-reinforced polycarbonate resin composition

    US20160024301A1