Perovskite quantum dot composite film and preparation method thereof

By using a polymer matrix formed by fluorinated acrylate and adhesion-promoting monomers in the perovskite quantum dot composite film, the problems of perovskite quantum dot stability and preparation complexity are solved, and high transparency and stability are achieved. , suitable for industrial production.

CN116001378BActive Publication Date: 2024-10-18CHINA LUCKY GROUP CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310141705.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-21
Publication Date
2024-10-18
Estimated Expiration
2043-02-21

AI Technical Summary

Technical Problem

Perovskite quantum dots have poor stability and are easily affected by water and oxygen. The polymer matrix used in the existing technology, such as PVDF, will affect the transparency and complicate the preparation process, and the hot pressing method may damage the quantum dots, making it difficult to achieve Industrial production.

Method used

It uses a polymer matrix formed by fluorine-containing acrylate monomers and adhesion-promoting monomers to improve the bonding strength between the perovskite quantum dot layer and the barrier layer through hydrogen bonding, simplify the film structure, reduce process steps, improve transparency and stability.

Benefits of technology

It improves the bonding stability, water resistance, weather resistance and transparency of the perovskite quantum dot composite film, simplifies the preparation process, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116001378B_ABST
    Figure CN116001378B_ABST
Patent Text Reader

Abstract

The present invention discloses a perovskite quantum dot composite film and a preparation method thereof. The perovskite quantum dot composite film comprises: a first barrier layer, a second barrier layer and a perovskite quantum dot layer, wherein the perovskite quantum dot layer is arranged on a surface of the first barrier layer, the perovskite quantum dot layer comprises perovskite quantum dots and a polymer matrix, and the monomers forming the polymer matrix comprise water-blocking monomers and adhesion-promoting monomers; the second barrier layer is arranged on the surface of the perovskite quantum dot layer away from the first barrier layer, wherein the water-blocking monomer comprises a fluorine-containing acrylate monomer, and the adhesion-promoting monomer comprises a group for combining with the first barrier layer and the second barrier layer to form a hydrogen bond. The perovskite quantum dot composite film not only has good bonding stability, water-blocking, weather resistance, optical properties and high transparency, but also has a simple film structure and a convenient production process, which is conducive to large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of display, and in particular, relates to a perovskite quantum dot composite film and a preparation method thereof. Background Art

[0002] In recent years, quantum dot materials have been increasingly used in the display field. Due to their narrow emission spectrum, they can significantly improve the color saturation of display devices. Compared with classic CdSe and InP quantum dots, perovskite quantum dots not only have higher luminous efficiency, but can also be prepared by in-situ methods, with simple preparation processes and low production costs. At the same time, in terms of environmental protection, perovskite quantum dots do not contain heavy metal cadmium and comply with EU RoHS standards. At present, perovskite quantum dots have become a research hotspot for luminescent materials in the display field and have huge market potential. Summary of the invention

[0003] The present invention is mainly proposed based on the following problems and findings:

[0004] Since perovskite quantum dots have poor stability and are easily affected by water and oxygen during use, they are generally encapsulated with a barrier layer. In order to improve the stability of perovskite quantum dots and the adhesion between the perovskite quantum dot layer and the barrier layer, some people have proposed using tetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), polyvinyl fluoride (PVF), etc. as polymer matrices to prepare a perovskite quantum dot composite film including an all-inorganic perovskite quantum dot layer, an upper water and oxygen barrier layer, a pressure-sensitive adhesive layer, and a lower water and oxygen barrier layer, wherein the pressure-sensitive adhesive layer is used to bond the all-inorganic perovskite quantum dot layer and the lower water and oxygen barrier layer. This method uses fluororesins such as PVDF as polymer matrices, and there is no adhesion between the fluororesins and the barrier layer. Therefore, a pressure-sensitive adhesive layer needs to be introduced between the all-inorganic perovskite quantum dot layer and the barrier layer for bonding, and the use of this fluororesin polymer will affect the transparency of the composite film, thereby reducing its light transmittance. For another example, some people have proposed to use PVDF, PMMA, polyacrylamide, bisphenol A epoxy acrylate, polyacrylonitrile, etc. as polymer matrices, at least a portion of at least one surface of the formed perovskite quantum dot-polymer layer is coated by a transition layer, and then a layer of oily acrylic pressure-sensitive adhesive is coated on the transition layer, and then compounded with the barrier layer. The multi-layer structure of the perovskite quantum dot composite film formed by this method at least includes a base layer, a quantum dot-polymer layer, a transition layer, an adhesive layer and a barrier layer. The number of film layers is large and the preparation process is complicated. For another example, some people have proposed to coat the PVDC source on the surface of the barrier layer to obtain a PVDC coating layer to improve the bonding force between the barrier layer and the perovskite quantum dot layer. However, the PVDC source used in this method is a PVDC emulsion. The emulsifier in the PVDC emulsion may have a destructive effect on the perovskite quantum dots and affect the stability of the perovskite quantum dots. In addition, in this method, before the barrier layer is coated with PVDC, the barrier layer needs to be treated with corona and primer, which increases the complexity of the process. For another example, some people have proposed using styrene-butadiene-styrene (SBS), styrene-ethylene / propylene-styrene (SEPS), and styrene-isoprene-styrene (SIS) as polymer matrices, mixing them with perovskite quantum dots and then coating them on a barrier layer to obtain a perovskite quantum dot composite film. However, the styrene hot-melt pressure-sensitive adhesive resin used in this method is not conducive to the growth of perovskite quantum dots in terms of molecular structure. Moreover, this method uses hot pressing to form the above-mentioned composite film. The hot pressing temperature is relatively high, which may damage the quantum dots. At the same time, the preparation process requires vacuum drying treatment, which is not conducive to industrial implementation.

[0005] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a perovskite quantum dot composite film and a preparation method thereof. The perovskite quantum dot composite film not only has good bonding stability, water barrier, weather resistance, optical properties and high transparency, but also has a simple film structure and a convenient production process, which is conducive to large-scale industrial production.

[0006] In one aspect of the present invention, the present invention provides a perovskite quantum dot composite film. According to an embodiment of the present invention, the composite film comprises:

[0007] First barrier layer;

[0008] A perovskite quantum dot layer, the perovskite quantum dot layer is disposed on one surface of the first barrier layer, the perovskite quantum dot layer comprises perovskite quantum dots and a polymer matrix, and the monomers forming the polymer matrix comprise a water-blocking monomer and an adhesion-promoting monomer;

[0009] a second barrier layer, wherein the second barrier layer is disposed on a surface of the perovskite quantum dot layer away from the first barrier layer,

[0010] The water-blocking monomer includes a fluorine-containing acrylate monomer, and the adhesion-promoting monomer includes a group for combining with the first barrier layer and the second barrier layer to form a hydrogen bond.

[0011] The perovskite quantum dot composite film according to the above embodiment of the present invention has at least the following beneficial effects: 1) A fluorine-containing acrylate monomer is introduced into the polymer matrix of the perovskite quantum dot layer so that the fluorine-containing acrylate polymer obtained by polymerization has good optical and electrical properties due to the small atomic radius, small polarizability, low refractive index and high electronegativity of the fluorine atom; on the other hand, since the fluorine-containing side chain groups in the polymer will undergo phase separation at the molecular level, the side chain fluorine-containing groups (such as fluorine-containing alkyl groups) extend outward from the polymer main chain and are arranged in a directional manner to form an ordered "comb-like" structure, and the electron cloud of the fluorine atom forms a "shielding protection" effect on the main chain and the internal molecules, thereby enhancing the stability of the main chain, which is beneficial to improving the water resistance, weather resistance and chemical inertness of the polymer matrix in the perovskite quantum dot layer, and enhancing the stability of the perovskite quantum dot composite film; on the other hand, Fluorine-containing acrylate polymers are also beneficial to the growth of perovskite quantum dots. At the same time, fluorine atoms can also form strong and uniform interactions with methylamine ions that form perovskite quantum dots. With the polymerization of fluorine-containing acrylates and the arrangement of polymer molecular chains, it is beneficial to enhance the dispersion effect of perovskite quantum dots in the polymer matrix, and promote the uniform distribution of perovskite quantum dots in the perovskite quantum dot layer; furthermore, since polyacrylate itself has good adhesion, it is also beneficial to improve the bonding strength between the perovskite quantum dot layer and the barrier layer, and enhance the protective effect of perovskite quantum dots; 2) By introducing adhesion-promoting monomers, the formed polymer matrix can contain groups that can combine with the first barrier layer and the second barrier layer to form hydrogen bonds. By forming hydrogen bonds between the perovskite quantum dot layer and the barrier layer, it is beneficial to improve the overall bonding strength of the perovskite quantum dot composite film, and further improve the stability of the perovskite quantum dot composite film.

[0012] In addition, the perovskite quantum dot composite film according to the above embodiment of the present invention may also have the following additional technical features:

[0013] In some embodiments of the present invention, the amount of the water-blocking monomer is not less than 5 wt % based on the total mass of the monomers forming the polymer matrix.

[0014] In some embodiments of the present invention, the amount of the adhesion promoting monomer is not less than 45 wt % based on the total weight of the monomers forming the polymer matrix.

[0015] In some embodiments of the present invention, the adhesion promoting monomer includes a hydroxyl-containing acrylate monomer and / or a furan ring-containing acrylate monomer.

[0016] In some embodiments of the present invention, the water-blocking monomer includes at least one of trifluoroethyl acrylate, trifluoroethyl methacrylate, hexafluoroisopropyl acrylate, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, octafluoropentyl acrylate, pentafluorophenyl acrylate, dodecafluoroheptyl acrylate, heptafluorobutyl acrylate, fluorooctyl ethyl acrylate, fluorooctyl methacrylate, fluorohexyl ethyl acrylate, and perfluorohexyl methacrylate.

[0017] In some embodiments of the present invention, the amount of the water-blocking monomer is 5-20 wt % based on the total weight of the monomers forming the polymer matrix.

[0018] In some embodiments of the present invention, the amount of the adhesion promoting monomer is 45-75 wt % based on the total weight of the monomers forming the polymer matrix.

[0019] In some embodiments of the present invention, the peeling force of the perovskite quantum dot composite film is 5 to 25 N / 25 mm.

[0020] In another aspect of the present invention, the present invention proposes a method for preparing the above-mentioned perovskite quantum dot composite film. According to an embodiment of the present invention, the method comprises: (1) mixing a water-blocking monomer, an adhesion-promoting monomer, an initiator and a first solvent to obtain a first mixed solution, and subjecting the first mixed solution to a polymerization reaction to obtain a polymer matrix solution; (2) mixing a precursor and a ligand for forming perovskite quantum dots with a second solvent to obtain a second mixed solution; (3) mixing the polymer matrix solution with the second mixed solution to obtain a perovskite quantum dot layer coating solution; (4) coating the perovskite quantum dot layer coating solution on a surface of the first barrier layer to obtain a perovskite quantum dot layer; (5) covering the second barrier layer on the surface of the perovskite quantum dot layer away from the first barrier layer to obtain a perovskite quantum dot composite film; wherein the water-blocking monomer comprises a fluorine-containing acrylate monomer, and the adhesion-promoting monomer comprises a group for combining with the first barrier layer and the second barrier layer to form a hydrogen bond.

[0021] Compared with the existing technology, this method is not only beneficial to improving the optical properties, bonding stability, water barrier properties, weather resistance and transparency of the perovskite quantum dot composite film, but also has a simple preparation process, which is conducive to industrial large-scale production.

[0022] In addition, the method for preparing a perovskite quantum dot composite film according to the above embodiment of the present invention may also have the following additional technical features:

[0023] In some embodiments of the present invention, in step (1), the mixing further comprises: adding a universal acrylate monomer.

[0024] In some embodiments of the present invention, the amount of the general acrylate monomer is 15-45 wt % based on the total weight of the monomers forming the polymer matrix.

[0025] In some embodiments of the present invention, the amount of the initiator is 0.5-6 wt % based on the total weight of the monomers forming the polymer matrix.

[0026] In some embodiments of the present invention, based on the total mass of the first mixed liquid, the amount of the first solvent is 65-85 wt %.

[0027] In some embodiments of the present invention, the initiator includes 2,2-azobisisobutyronitrile and / or benzoyl peroxide.

[0028] In some embodiments of the present invention, the first solvent comprises ethyl acetate.

[0029] In some embodiments of the present invention, in step (2), the precursor includes a first precursor and a second precursor, the first precursor includes a compound with a chemical formula of PbX2 type, and the second precursor includes a metal halide with a chemical formula of AX type, wherein A includes at least one of CH3NH2, CH(NH)NH2, and Cs, and X includes at least one of F, Cl, Br, and I.

[0030] In some embodiments of the present invention, the ligand includes at least one of butylamine, n-octylamine, dodecylamine, oleylamine, oleic acid, 2,2-dicarboxydiphenylamine, alkylphosphinic acid, alkylphosphinic acid, 3,3-diphenylpropylamine, n-dodecyl mercaptan, trioctylphosphine, and trioctylphosphine oxide.

[0031] In some embodiments of the present invention, the second solvent includes N,N-dimethylformamide.

[0032] In some embodiments of the present invention, based on the total mass of the second mixed liquid, the amount of the first precursor is 2-20wt%, the amount of the second precursor is 2-5wt%, the amount of the ligand is 1-5wt%, and the amount of the second solvent is 70-95wt%.

[0033] In some embodiments of the present invention, in step (3), based on the total mass of the perovskite quantum dot layer coating liquid, the content of the second mixed liquid is 0.1 to 5 wt %.

[0034] In another aspect of the present invention, the present invention proposes a display device. According to an embodiment of the present invention, the display device is prepared using the above-mentioned perovskite quantum dot composite film and / or the perovskite quantum dot composite film obtained by the above-mentioned method. Compared with the prior art, the display device has all the technical features and effects of the above-mentioned perovskite quantum dot composite film and the above-mentioned method for preparing the perovskite quantum dot composite film, which will not be repeated here. In general, the display device not only has a simple preparation process, but also has high luminous efficiency, good stability in use, and low cost.

[0035] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0037] Figure 1 is a schematic structural diagram of a perovskite quantum dot composite film according to an embodiment of the present invention;

[0038] Figure 2 is a flow chart of a method for preparing a perovskite quantum dot composite film according to one embodiment of the present invention;

[0039] Figure 3 This is an emission spectrum curve of the perovskite quantum dot composite film according to Example 2 of the present invention.

[0040] Reference numerals:

[0041] 10-first barrier layer; 11-side of the first barrier layer away from the perovskite quantum dot layer; 12-side of the first barrier layer in contact with the perovskite quantum dot layer; 20-perovskite quantum dot layer; 21-perovskite quantum dots; 22-polymer matrix; 30-second barrier layer; 31-side of the second barrier layer away from the perovskite quantum dot layer; 32-side of the second barrier layer in contact with the perovskite quantum dot layer. DETAILED DESCRIPTION

[0042] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limitations on the present invention. In the description of the present invention, it should be understood that the terms "first" and "second" are used only for descriptive purposes, and should not be construed as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0043] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0044] In one aspect of the present invention, the present invention provides a perovskite quantum dot composite film. According to an embodiment of the present invention, in combination with Figure 1 It is understood that the composite film includes: a first barrier layer 10, a perovskite quantum dot layer 20 and a second barrier layer 30, the perovskite quantum dot layer 20 is arranged on a surface of the first barrier layer 10, the perovskite quantum dot layer 20 includes perovskite quantum dots 21 and a polymer matrix 22, and the monomers forming the polymer matrix 22 include water-blocking monomers and adhesion-promoting monomers; the second barrier layer 30 is arranged on the surface of the perovskite quantum dot layer 20 away from the first barrier layer 10, wherein the water-blocking monomer includes a fluorine-containing acrylate monomer, and the adhesion-promoting monomer includes a group for combining with the first barrier layer and the second barrier layer to form hydrogen bonds.

[0045] The perovskite quantum dot composite film according to the above embodiment of the present invention has at least the following beneficial effects: 1) A fluorine-containing acrylate monomer is introduced into the polymer matrix of the perovskite quantum dot layer so that the fluorine-containing acrylate polymer obtained by polymerization has good optical and electrical properties due to the small atomic radius, small polarizability, low refractive index and high electronegativity of the fluorine atom; on the other hand, since the fluorine-containing side chain groups in the polymer will undergo phase separation at the molecular level, the side chain fluorine-containing groups (such as fluorine-containing alkyl groups) extend outward from the polymer main chain and are arranged in a directional manner to form an ordered "comb-like" structure, and the electron cloud of the fluorine atom forms a "shielding protection" effect on the main chain and the internal molecules, thereby enhancing the stability of the main chain, which is beneficial to improving the water resistance, weather resistance and chemical inertness of the polymer matrix in the perovskite quantum dot layer, and enhancing the stability of the perovskite quantum dot composite film; on the other hand, Fluorine-containing acrylate polymers are also beneficial to the growth of perovskite quantum dots. At the same time, fluorine atoms can also form strong and uniform interactions with methylamine ions that form perovskite quantum dots. With the polymerization of fluorine-containing acrylates and the arrangement of polymer molecular chains, it is beneficial to enhance the dispersion effect of perovskite quantum dots in the polymer matrix, and promote the uniform distribution of perovskite quantum dots in the perovskite quantum dot layer; furthermore, since polyacrylate itself has good adhesion, it is also beneficial to improve the bonding strength between the perovskite quantum dot layer and the barrier layer, and enhance the protective effect of perovskite quantum dots; 2) By introducing adhesion-promoting monomers, the formed polymer matrix can contain groups that can combine with the first barrier layer and the second barrier layer to form hydrogen bonds. By forming hydrogen bonds between the perovskite quantum dot layer and the barrier layer, it is beneficial to improve the overall bonding strength of the perovskite quantum dot composite film, and further improve the stability of the perovskite quantum dot composite film.

[0046] According to an embodiment of the present invention, based on the total mass of the monomers forming the polymer matrix, the amount of the water-repellent monomer may be no less than 5wt%, for example, it may be 8wt%, 10wt%, 15wt%, 20wt%, 30wt%, 40wt% or 60wt%, etc. The inventors have found that if the amount of the water-repellent monomer is too small, the fluorine atom content in the formed polymer matrix is ​​too small, which will not only affect the growth of the perovskite quantum dots and their dispersion effect, but also be unfavorable for improving the water-repellent, weather resistance and chemical inertness of the polymer matrix in the perovskite quantum dot layer, and is not conducive to enhancing the protective effect of the polymer matrix on the perovskite quantum dot layer, and is not conducive to improving the stability of the perovskite quantum dot composite film. Further, according to some specific examples of the present invention, based on the total mass of the monomers that form the polymer matrix, the amount of the water-blocking monomer can be 5 to 20 wt%, for example, 6 wt%, 9 wt%, 12 wt%, 16 wt% or 18 wt%, etc. The inventors found that if the amount of the water-blocking monomer is too much, it will not only be difficult to further significantly improve the water barrier and weather resistance of the polymer matrix, but also lead to an increase in production costs. The present invention controls the amount of the water-blocking monomer within the above range, which is not only conducive to promoting the growth and dispersion of perovskite quantum dots and improving the stability of perovskite quantum dots, but also can further control processing costs. It should be noted that the specific type of water-blocking monomer is not particularly limited in the present invention, and those skilled in the art can flexibly select it according to actual conditions. For example, the water-blocking monomer may include at least one of trifluoroethyl acrylate, trifluoroethyl methacrylate, hexafluoroisopropyl acrylate, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, octafluoropentyl acrylate, pentafluorophenyl acrylate, dodecafluoroheptyl acrylate, heptafluorobutyl acrylate, fluorooctyl ethyl acrylate, fluorooctyl methacrylate, fluorohexyl ethyl acrylate, and perfluorohexyl methacrylate.

[0047] According to an embodiment of the present invention, based on the total mass of the monomers forming the polymer matrix, the amount of the adhesion promoting monomer may be no less than 45wt%, for example, 48wt%, 55wt%, 60wt%, 70wt%, 80wt% or 90wt%, etc. The inventors have found that if the amount of the adhesion promoting monomer is too small, it is not conducive to improving the bonding strength between the polymer matrix and the barrier layer, and affects the water and oxygen barrier effect of the barrier layer on the perovskite quantum dot layer. Further, according to some specific examples of the present invention, based on the total mass of the monomers forming the polymer matrix, the amount of the adhesion promoting monomer may be 45-75wt%, for example, 50wt%, 58wt%, 65wt% or 72wt%, etc. The inventors have found that if the amount of the adhesion promoting monomer is too much, it may lead to a reduction in the amount of the water-blocking monomer, which is not only easy to affect the growth of the perovskite quantum dots, but also not conducive to improving the water barrier, weather resistance and chemical inertness of the polymer matrix in the perovskite quantum dot layer, and affecting the stability of the perovskite quantum dots. The present invention controls the amount of the adhesion-promoting monomer within the above range, which is beneficial to taking into account the water resistance, weather resistance and bonding stability of the perovskite quantum dot composite film. It should be noted that there is no particular restriction on the specific type of the adhesion-promoting monomer in the present invention, and those skilled in the art can flexibly select it according to actual conditions. It is preferably an acrylate monomer containing a hydroxyl group and / or a furan ring, for example, it can include at least one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, tetrahydrofuran methacrylate, 2-hydroxyethyl methacrylate phosphate, and 4-hydroxybutyl acrylate, thereby increasing the content of the acrylate segment in the polymer matrix and further enhancing the bonding strength of the perovskite quantum dot layer and the barrier layer.

[0048] According to an embodiment of the present invention, the monomers forming the polymer matrix may also include general acrylate monomers, thereby not only facilitating the uniform distribution of the segments formed by the water-blocking monomers and the adhesion-promoting monomers in the total segments of the polymer matrix, improving the water-blocking property of the perovskite quantum dot layer and the adhesion to the barrier layer, but also reducing the cost of raw materials. Further, according to some specific examples of the present invention, based on the total mass of the monomers forming the polymer matrix, the amount of general acrylate monomers may be 15 to 45 wt%, for example, 20 wt%, 25 wt%, 30 wt%, 35 wt% or 40 wt%, etc. The inventors have found that if the amount of general acrylate is too little, the cost of raw materials increases; if the amount of general acrylate is too much, it will affect the water-blocking and bonding stability of the perovskite quantum dot composite film. The present invention controls the amount of general acrylate monomers within the above range, which is conducive to taking into account both the production cost and the stability of the composite film. It should be noted that there is no particular limitation on the specific type of the general acrylate monomer in the present invention, and those skilled in the art can flexibly select it according to actual conditions. For example, it may include at least one of methyl acrylate, ethyl acrylate, butyl acrylate, and octyl acrylate.

[0049] According to an embodiment of the present invention, the perovskite quantum dot composite film of the present invention is prepared by adding a water-blocking monomer to a polymer matrix, and a fluorine-containing acrylate polymer is introduced into the polymer matrix, which is not only conducive to promoting the in-situ growth of the perovskite quantum dots in the polymer matrix, reducing the damage of water and oxygen to the perovskite quantum dots, and enhancing its stability in use, but also can improve the transparency of the composite film; on the other hand, by introducing an adhesion-promoting monomer to prepare a polymer matrix, it is conducive to improving the bonding strength between the perovskite quantum dot layer and the barrier layer, so that the perovskite quantum dot layer can be directly bonded to the barrier layer, which can reduce the number of layers of the composite film, and there is no need to perform surface treatment processes such as corona or primer coating on the barrier layer, which can not only It can reduce the cost of raw materials and processes, and can also solve the problem of poor adhesion between the existing perovskite quantum dot layer and the barrier layer. Specifically, the peeling force of the perovskite quantum dot composite film prepared by the above method of the present invention can be no less than 5N / 25mm, for example, it can reach 5-25N / 25mm, specifically 7N / 25mm, 10N / 25mm, 13N / 25mm, 15N / 25mm, 18N / 25mm, 21N / 25mm or 24N / 25mm, etc., thereby meeting the bonding requirements of the perovskite quantum dot layer and the barrier layer, avoiding or reducing the entry of water and oxygen into the bonding interface between the perovskite quantum dot layer and the barrier layer to affect the stability of the perovskite quantum dots.

[0050] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned perovskite quantum dot composite film. Figure 2 It is understood that according to an embodiment of the present invention, the method includes:

[0051] S100: mixing a water-blocking monomer, an adhesion-promoting monomer, an initiator and a first solvent to obtain a first mixed solution, and subjecting the first mixed solution to a polymerization reaction to obtain a polymer matrix solution.

[0052] According to an embodiment of the present invention, the water-blocking monomer, the adhesion-promoting monomer, the initiator and the first solvent are mixed, so that the water-blocking monomer and the adhesion-promoting monomer are dispersed in the solution, and a copolymerization reaction occurs under the catalytic promotion of the initiator, so that a polymer including a fluorinated acrylate segment can be obtained, and the polymer contains a group that can form a hydrogen bond with the barrier layer, such as a hydroxyl group, a furan ring, etc. Among them, the selection type, function and dosage of the water-blocking monomer and the adhesion-promoting monomer in the present invention have been described in detail in the previous part, and will not be repeated here. In addition, according to some specific examples of the present invention, based on the total mass of the monomers forming the polymer matrix, the amount of the initiator can be 0.5 to 6wt%, for example, 1wt%, 2wt%, 3wt%, 4wt% or 5wt%, etc. The inventors found that if the amount of the initiator is too little, the polymerization reaction speed will be slow, and it will even be difficult to make the monomer react completely; if the amount of the initiator is too much, the risk of reaction explosion will increase. The present invention controls the amount of the initiator within the above range, which is conducive to controlling the polymerization reaction to proceed smoothly. In addition, based on the total mass of the first mixed solution, the amount of the first solvent can be 65-85wt%, for example, 70wt%, 75wt% or 80wt%, etc. The inventors found that if the amount of the first solvent is too small, the concentration of the monomer and the initiator in the first mixed solution is too high, which is also easy to cause implosion and poses a safety hazard; if the amount of the first solvent is too much, on the one hand, it will lead to a decrease in reaction efficiency and even cause insufficient reaction degree, and on the other hand, it is also a waste of resources. The present invention is also beneficial to control the rate and degree of the polymerization reaction by controlling the amount of the first solvent within the above range. It should be noted that there is no particular restriction on the specific types of the initiator and the first solvent in the present invention, and those skilled in the art can flexibly choose according to actual conditions. For example, the initiator can be 2,2-azobisisobutyronitrile and / or benzoyl peroxide; the first solvent can include ethyl acetate, etc.

[0053] According to an embodiment of the present invention, a general acrylate monomer may be added during the above mixing process, wherein the selection type, function and dosage of the acrylate are also described in detail in the previous section and will not be repeated here.

[0054] According to the embodiments of the present invention, there is no particular restriction on the specific conditions of the mixing process and the polymerization process of the first mixed solution in the present invention, and those skilled in the art can flexibly select according to the actual situation. For example, before the polymerization, a protective gas, such as at least one of nitrogen, argon, and helium, is introduced into the reaction system (the first mixed solution), and the flow rate of the protective gas can be controlled to be 1 to 10 mL / min, the temperature of the polymerization reaction can be 50 to 80°C, and the time can be 8 to 24 hours, which is beneficial to taking into account both the efficiency and reaction degree of the polymerization reaction and obtaining a relatively complete polymer matrix.

[0055] S200: Mixing the precursor and ligand for forming perovskite quantum dots with the second solvent to obtain a second mixed solution

[0056] According to an embodiment of the present invention, by mixing the precursor and ligand used to form perovskite quantum dots in a second solvent, a second mixed solution, i.e., a perovskite quantum dot precursor solution, can be obtained. Wherein, the precursor used to form perovskite quantum dots may include a first precursor and a second precursor, the first precursor may include a compound with a chemical formula of PbX2 type, and the second precursor may include a metal halide with a chemical formula of AX type, wherein A may include at least one of CH3NH2, CH(NH)NH2, and Cs, and X may include at least one of F, Cl, Br, and I. In addition, there is no particular restriction on the specific type of ligand in the present invention, and those skilled in the art may flexibly select according to actual conditions, for example, the ligand may include at least one of butylamine, n-octylamine, dodecylamine, oleylamine, oleic acid, 2,2-dicarboxydiphenylamine, alkylphosphinic acid, alkylphosphinic acid, 3,3-diphenylpropylamine, n-dodecyl mercaptan, trioctylphosphine, and trioctylphosphine oxide. In addition, there is no particular limitation on the specific type of the second solvent in the present invention, as long as it is miscible with the polymer matrix solution, for example, it can be N,N-dimethylformamide, etc., thereby achieving the growth of perovskite quantum dots in the polymer matrix in the same system.

[0057] According to an embodiment of the present invention, based on the total mass of the second mixed liquid, the amount of the first precursor can be 2-20wt%, for example, 5wt%, 12wt%, 15wt% or 18wt%, etc.; the amount of the second precursor can be 2-5wt%, for example, 3wt%, 3.5wt%, 4wt% or 4.5wt%, etc.; the amount of the ligand can be 1-5wt%, for example, 1.5wt%, 2wt%, 3wt% or 4wt%, etc.; the amount of the second solvent can be 70-95wt%, for example, 75wt%, 80wt%, 85wt% or 90wt%, etc. The inventors found that if the amount of the first precursor is too much or the amount of the second precursor is too little, the subsequent perovskite quantum dot layer coating liquid may have excess first precursor precipitated as solid during the film formation process; if the amount of the second precursor is too much or the amount of the first precursor is too little, the subsequent perovskite quantum dot layer coating liquid may have excess second precursor precipitated as solid during the film formation process, both of which will affect the growth of perovskite quantum dots and the stability of the perovskite quantum dot layer; in addition, the inventors found that if the amount of the second solvent is too little, it may lead to incomplete dissolution of the precursor, and if the amount of the second solvent is too much, it will hinder or slow down the film formation efficiency of the perovskite quantum dot layer. The present invention is conducive to promoting the growth stability of perovskite quantum dots by controlling the amount of the first precursor, the second precursor, the ligand and the second solvent within the above range.

[0058] S300: Mixing the polymer matrix solution with the second mixed solution to obtain a perovskite quantum dot layer coating solution

[0059] According to an embodiment of the present invention, the perovskite quantum dot coating liquid includes a polymer matrix solution (including a polymer matrix and a first solvent) and a second mixed liquid (including a perovskite quantum dot precursor and a second solvent). Based on the total mass of the perovskite quantum dot layer coating liquid, the content of the second mixed liquid can be 0.1-5wt%, for example, 0.5wt%, 1wt%, 2wt%, 3wt% or 4wt%, etc. The inventor found that when the amount of the second mixed liquid is too small, the content of perovskite quantum dots in the formed perovskite quantum dot layer is too small, and it is difficult to achieve an effective luminescence effect; if the amount of the second mixed liquid is too much, the concentration of the precursor in the perovskite quantum dot layer coating liquid is high, and it is easy to agglomerate, which affects the growth of the perovskite quantum dots. The present invention controls the amount of the second mixed liquid in the perovskite quantum dot layer coating liquid within the above range, which is conducive to taking into account the growth and luminescence effect of the perovskite quantum dots.

[0060] S400: coating the perovskite quantum dot layer coating liquid onto one surface of the first barrier layer to obtain a perovskite quantum dot layer

[0061] According to an embodiment of the present invention, after the perovskite quantum dot layer coating liquid is coated on a surface of the first barrier layer, the perovskite quantum dots can be crystallized and grown in the polymer matrix. Specifically, the coated first barrier layer can be dried. As the solvent in the coating liquid evaporates, due to the hydrogen bonding between the precursor molecules of the perovskite quantum dots, when the critical nucleation concentration is reached, the precursor molecules will self-assemble, the inorganic metal cations can form coordinated octahedra with the halogen anions, and the organic amine cations can enter the pores between adjacent octahedra to form a hybrid perovskite structure. At the same time, as the solvent decreases, the chain segment movement of the polymer matrix is ​​gradually restricted, and it will be coated on the surface of the formed perovskite particles, limiting the growth of the perovskite particles in the three-dimensional direction, and limiting the particle size to the nanometer level, thereby obtaining a perovskite quantum dot layer. It should be noted that in the present invention, there are no special restrictions on the coating method, drying method and thickness of the formed perovskite quantum dot layer of the perovskite quantum dot layer coating liquid. Those skilled in the art can flexibly select according to actual conditions. For example, the coating method can be comma blade coating, gravure coating, micro-gravure coating, etc.; the coating speed can be 1-5 m / s; the drying temperature can be 25-80°C, and the drying method can be to dry and solidify the first barrier layer coated with the perovskite quantum dot layer coating liquid in four temperature ranges in turn; the thickness of the finally formed perovskite quantum dot layer can be 1-20 μm.

[0062] S500: Covering the second barrier layer on the surface of the perovskite quantum dot layer away from the first barrier layer to obtain a perovskite quantum dot composite film

[0063] According to an embodiment of the present invention, after the second barrier layer is covered on the surface of the perovskite quantum dot layer away from the first barrier layer, a perovskite quantum dot composite film can be obtained by pressing treatment. In the present invention, there are no special restrictions on the specific conditions of the pressing treatment and the thickness of the perovskite quantum dot composite film after the pressing treatment. Those skilled in the art can flexibly select according to actual conditions. For example, the pressing force can be 0.1 to 0.5 MPa, and the thickness of the composite film can be 101 to 420 μm.

[0064] According to an embodiment of the present invention, Figure 1 It is understood that the first barrier layer 10 and the second barrier layer 30 may be in contact with the perovskite quantum dot layer 20 on one side or the other side. Figure 1 12 and 32), the side away from the perovskite quantum dot layer can be a diffusion surface (combined with Figure 1 In addition, the present invention has no particular restrictions on the specific material, thickness and water and oxygen permeability of the barrier layer, and those skilled in the art can flexibly select them according to actual conditions. For example, the water vapor permeability of the first barrier layer and the second barrier layer can be independently (10 -2~10 -1 )g / m 2 / day, and the oxygen permeability can be independently (10 -2 ~10 -1 )mL / m 2 / day, the thickness can be 50-200 μm respectively, and the material of the first barrier layer and the second barrier layer can independently include at least one of Al2O3 and SiO2.

[0065] In summary, the method for preparing a perovskite quantum dot composite film according to the above embodiment of the present invention, compared with the prior art, is not only beneficial to improving the optical properties, bonding stability, water resistance, weather resistance and transparency of the perovskite quantum dot composite film, but also has a simple preparation process, which is conducive to realizing industrial large-scale production.

[0066] In another aspect of the present invention, the present invention proposes a display device. According to an embodiment of the present invention, the display device is prepared by using the above-mentioned perovskite quantum dot composite film and / or the perovskite quantum dot composite film obtained by the above-mentioned method. Compared with the prior art, the display device has all the technical features and effects of the above-mentioned perovskite quantum dot composite film and the above-mentioned method for preparing the perovskite quantum dot composite film, which will not be repeated here. In general, the display device not only has a simple preparation process, but also has high luminous efficiency, good stability in use, and low cost.

[0067] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.

[0068] Example 1

[0069] (1) Commercially available butyl acrylate (BA), hydroxyethyl acrylate (HEA), and hexafluoroisopropyl acrylate (HFIA) raw materials were purified by vacuum distillation, 84 g of the purified butyl acrylate (BA), 226 g of hydroxyethyl acrylate (HEA), and 40 g of hexafluoroisopropyl acrylate (HFIA) were added to a reaction flask, 4.5 g of azobisisobutyronitrile (AIBN) and 1200 g of ethyl acetate (EA) were added thereto, and mechanical stirring was performed at a speed of 500 r / min to obtain a first mixed solution, nitrogen was introduced into the reaction flask at a flow rate of 1 mL / min to purge residual air in the system, and after 2 hours, the first mixed solution was heated to 58° C. to start the reaction, and after 4 hours, the temperature of the first mixed solution was raised to 60° C. to continue the reaction, and the material was discharged after 12 hours to obtain 1500 g of a polymer matrix solution;

[0070] (2) 14.2 g of lead bromide, 3.6 g of cesium bromide, 2.4 g of methylamine bromide, 4.8 g of 3,3-diphenylpropylamine, and 175 g of N,N-dimethylformamide were mixed and stirred at room temperature to completely dissolve the solid to obtain 200 g of a second mixed solution;

[0071] (3) adding 15 g of the second mixed solution to 1500 g of the polymer matrix solution prepared in step (1), and mechanically stirring at a speed of 500 r / min for 6 h to obtain a perovskite quantum dot layer coating solution; coating the perovskite quantum dot layer coating solution on the barrier surface of the first barrier layer by comma coating, with a wet film thickness of 50 μm and a coating speed of 5 m / s; drying in a drying channel at temperatures of 50° C., 55° C., 60° C., and 65° C., and then laminating the barrier surface of the second barrier layer at a pressure of 0.2 MPa at a winding position to obtain a perovskite quantum dot composite film with a thickness of 270 μm.

[0072] Example 2

[0073] The difference from Example 1 is that in step (1), the amount of refined butyl acrylate used is 79 g, the amount of hydroxyethyl acrylate used is 211 g, and the amount of hexafluoroisopropyl acrylate used is 60 g.

[0074] Example 3

[0075] The difference from Example 1 is that in step (1), the amount of refined butyl acrylate used is 129 g, the amount of hydroxyethyl acrylate used is 170 g, and the amount of hexafluoroisopropyl acrylate used is 51 g.

[0076] Example 4

[0077] The difference from Example 1 is that in step (1), the amount of refined butyl acrylate used is 93 g, the amount of hydroxyethyl acrylate used is 220 g, and the amount of hexafluoroisopropyl acrylate used is 37 g.

[0078] Example 5

[0079] The difference from Example 1 is that in step (1), the amount of refined butyl acrylate used is 76 g, the amount of hydroxyethyl acrylate used is 204 g, and the amount of hexafluoroisopropyl acrylate used is 70 g.

[0080] Example 6

[0081] The difference from Example 1 is that in step (1), the amount of refined butyl acrylate used is 150 g, the amount of hydroxyethyl acrylate used is 140 g, and the amount of hexafluoroisopropyl acrylate used is 60 g.

[0082] Comparative Example 1

[0083] The difference from Example 1 is that step (1) is: dissolving 350 g of polyvinylidene fluoride (PVDF) in 1150 g of DMF, and mechanically stirring to mix them evenly to obtain 1500 g of polymer matrix solution.

[0084] Testing and analysis

[0085] Under the same conditions, the perovskite quantum dot composite films prepared in Examples 1 to 6 and Comparative Example 1 were characterized by the following test methods, including: peeling force of the perovskite quantum dot composite film, emission spectrum of the perovskite quantum dot composite film before and after aging, and failure edge of the perovskite quantum dot composite film after aging. The specific steps of aging the embodiments 1 to 6 and Comparative Example 1 are as follows: under the same conditions, the perovskite quantum dot composite film samples prepared in the above embodiments 1 to 6 and Comparative Example 1 were cut into 10 cm × 10 cm size pieces, and placed in a constant temperature and humidity chamber at 60°C and 90% RH for continuous aging for 500 hours.

[0086] Failure edge: After the aged perovskite quantum dot composite film is taken out, its failure edge is measured with a scaled magnifying glass;

[0087] The perovskite quantum dot composite film was cut into 200 mm × 25 mm, the peeling speed was 300 mm / min, and a 180-degree peeling test was performed using a tensile testing machine to obtain the peeling force value.

[0088] The test results of the peeling force of the perovskite quantum dot composite films prepared in Examples 1 to 6 and Comparative Example 1 and the failure edge of the aged perovskite quantum dot composite films are shown in Table 1.

[0089] Table 1 Peeling force and failure edge test results of the perovskite quantum dot composite films prepared in Examples 1 to 6 and Comparative Example 1

[0090]

[0091] Results and Discussion

[0092] The perovskite quantum dot composite films prepared in the examples and comparative examples were subjected to aging analysis. According to the emission spectra of the perovskite quantum dot composite films before and after aging, it can be seen that the perovskite quantum dot composite films prepared in the above examples of the present invention have good aging resistance stability. For example, taking the composite film prepared in Example 2 as an example, Figure 3 The two curves are emission spectra of the perovskite quantum dot composite film prepared in Example 2 before and after aging. Figure 3 It can be seen that the emission spectrum peak of the composite film before aging is at 525nm, and the half-width is 24nm, which is relatively narrow; the emission spectrum of the composite film after aging does not show significant changes compared with that before aging, indicating that the perovskite quantum dot composite film has good aging resistance and stability.

[0093] In addition, it can be seen from the data in Table 1 that, compared with Comparative Example 1, Examples 1 to 6 can have a higher peel strength by adopting the perovskite quantum dot composite film of the above-mentioned embodiment of the invention while maintaining the failure edge after aging without significant increase. Further, it can be seen from Table 1 that with the increase in the amount of water-blocking monomer (taking HFIA as an example), the failure edge decreases, indicating that the addition of water-blocking monomers can effectively improve the long-term use stability of the perovskite quantum dot composite film; in addition, with the increase in the amount of adhesion-promoting monomers (taking HEA as an example), the peeling force increases, and the addition of surface adhesion-promoting monomers can effectively enhance the bonding strength of the perovskite quantum dot composite film. Those skilled in the art can flexibly adjust the amount of water-blocking monomers and adhesion-promoting monomers in the polymer matrix according to actual needs, thereby obtaining a perovskite quantum dot composite film with good peeling force and / or failure edge.

[0094] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0095] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A perovskite quantum dot composite film, characterized in that: include: First barrier layer; A perovskite quantum dot layer, wherein the perovskite quantum dot layer is disposed on one surface of the first barrier layer, the perovskite quantum dot layer comprises perovskite quantum dots and a polymer matrix, and the monomers forming the polymer matrix comprise a water-blocking monomer and an adhesion-promoting monomer; a second barrier layer, wherein the second barrier layer is disposed on a surface of the perovskite quantum dot layer away from the first barrier layer, wherein the water-blocking monomer comprises a fluorine-containing acrylate monomer, and the adhesion-promoting monomer comprises a group for forming hydrogen bonds with the first barrier layer and the second barrier layer; The adhesion promoting monomer includes a hydroxyl-containing acrylate monomer and / or a furan ring-containing acrylate monomer; Based on the total weight of monomers forming the polymer matrix, the amount of the water-blocking monomer is not less than 5wt%; the amount of the adhesion-promoting monomer is not less than 45wt%.

2. The perovskite quantum dot composite film according to claim 1, characterized in that: The water-blocking monomer includes at least one of trifluoroethyl acrylate, trifluoroethyl methacrylate, hexafluoroisopropyl acrylate, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, octafluoropentyl acrylate, pentafluorophenyl acrylate, dodecafluoroheptyl acrylate, heptafluorobutyl acrylate, fluorooctyl ethyl acrylate, fluorooctyl methacrylate, fluorohexyl ethyl acrylate, and perfluorohexyl methacrylate.

3. The perovskite quantum dot composite film according to claim 1, characterized in that: Based on the total weight of the monomers forming the polymer matrix, the amount of the water-blocking monomer is 5-20 wt %; and / or the amount of the adhesion-promoting monomer is 45-75 wt %.

4. The perovskite quantum dot composite film according to any one of claims 1 to 3, characterized in that The peeling force of the perovskite quantum dot composite film is 5~25N / 25mm.

5. A method for preparing the perovskite quantum dot composite film according to any one of claims 1 to 4, characterized in that: include: (1) mixing a water-blocking monomer, an adhesion-promoting monomer, an initiator, and a first solvent to obtain a first mixed solution, and subjecting the first mixed solution to a polymerization reaction to obtain a polymer matrix solution; (2) mixing a precursor and a ligand for forming perovskite quantum dots with a second solvent to obtain a second mixed solution; (3) mixing the polymer matrix solution with the second mixed solution to obtain a perovskite quantum dot layer coating solution; (4) coating the perovskite quantum dot layer coating solution onto one surface of the first barrier layer to obtain a perovskite quantum dot layer; (5) covering the surface of the perovskite quantum dot layer away from the first barrier layer with a second barrier layer to obtain a perovskite quantum dot composite film; The water-blocking monomer includes a fluorine-containing acrylate monomer, and the adhesion-promoting monomer includes a group for combining with the first barrier layer and the second barrier layer to form a hydrogen bond.

6. The method according to claim 5, characterized in that In step (1), the mixing further comprises: adding a general acrylate monomer; Optionally, the amount of the general acrylate monomer is 15-45wt% based on the total mass of the monomers forming the polymer matrix; Optionally, the amount of the initiator is 0.5-6wt% based on the total mass of the monomers forming the polymer matrix; Optionally, based on the total mass of the first mixed solution, the amount of the first solvent is 65-85wt%; Optionally, the initiator comprises 2,2-azobisisobutyronitrile and / or benzoyl peroxide; Optionally, the first solvent comprises ethyl acetate.

7. The method according to claim 5, in step (2), the precursor comprises a first precursor and a second precursor, the first precursor comprises a compound with a chemical formula of PbX2 type, the second precursor comprises a metal halide with a chemical formula of AX type, wherein: A includes at least one of CH3NH2, CH(NH)NH2, and Cs, and X includes at least one of F, Cl, Br, and I; Optionally, the ligand includes at least one of butylamine, n-octylamine, dodecylamine, oleylamine, oleic acid, 2,2-dicarboxydiphenylamine, alkylphosphinic acid, 3,3-diphenylpropylamine, n-dodecylmercaptan, trioctylphosphine, and trioctylphosphine oxide; Optionally, the second solvent comprises N,N-dimethylformamide; Optionally, based on the total mass of the second mixed liquid, the amount of the first precursor is 2-20wt%, the amount of the second precursor is 2-5wt%, the amount of the ligand is 1-5wt%, and the amount of the second solvent is 70-95wt%.

8. The method according to claim 5, characterized in that In step (3), based on the total mass of the perovskite quantum dot layer coating liquid, the content of the second mixed liquid is 0.1-5wt%.

9. A display device, characterized in that: The perovskite quantum dot composite film is prepared by using the perovskite quantum dot composite film according to any one of claims 1 to 4 and / or the perovskite quantum dot composite film obtained by the method according to any one of claims 6 to 8.

Citation Information

Patent Citations

  • Perovskite quantum dot membrane, quantum dot diffusion composite membrane and preparation method of quantum dot diffusion composite membrane

    CN107955199A

  • High-stability all-inorganic perovskite quantum dot film and preparation method thereof

    CN109795172A

  • Perovskite quantum dot glue preparation method

    CN110845976A

  • Composite material and preparation method thereof and quantum dot light emitting diode

    CN111640876A

  • Quantum dot ink, preparation method of quantum dot light emitting diode and display device

    CN112646418A