A hard carbon material with core-shell structure and its preparation method and application

By using a core-shell structure material with a cross-linked porous structure hard carbon core and a dense carbon outer shell in lithium-ion batteries, the problems of low Coulombic efficiency and insufficient rate performance of hard carbon materials in lithium-ion batteries are solved for the first time, and efficient lithium-ion batteries are realized. Ion transmission and capacity retention simplify the process and are suitable for large-scale production.

CN116014102BActive Publication Date: 2024-10-29NINGBO UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211717628.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-29
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

For the first time in lithium-ion batteries, existing hard carbon materials suffer from low Coulombic efficiency, insufficient irreversible capacity and rate performance, and the carbon coating process is complex, consumes large amounts of energy, and easily leads to increased lithium ion diffusion resistance.

Method used

Using a core-shell structural material with a cross-linked porous structure of hard carbon core and dense carbon shell, polyacrylonitrile and sodium alginate are used as carbonaceous precursors, combined with high temperature treatment, rapid cooling, pre-oxidation and carbonization treatment to form a stable The core-shell structure avoids the problem of pore clogging during the carbon coating process.

Benefits of technology

It achieves high reversible capacity, high rate performance and high first-time Coulombic efficiency. The first-time Coulombic efficiency reaches 92%, the reversible capacity reaches 560mAh/g, the capacity does not decay after 1,000 cycles at 1 C, and the process is simple and can be mass-produced on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116014102B_ABST
    Figure CN116014102B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of lithium ion batteries, and specifically relates to a hard carbon material with a core-shell structure, a preparation method thereof and an application thereof. The hard carbon material has a core of hard carbon with a cross-linked porous structure and an outer shell of a dense carbon layer. The preparation method thereof includes preparing a polyacrylonitrile solution and a sodium alginate solution, mixing the polyacrylonitrile solution and the sodium alginate solution, high temperature treatment, rapid cooling, pre-oxidation treatment and carbonization treatment, and is used as a negative electrode active material for lithium ion batteries, which can obtain high reversible capacity, high rate performance and high first coulomb efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a hard carbon material with a core-shell structure and a preparation method and application thereof. Background Art

[0002] The refueling-style charging of electric vehicles requires that their core electrochemical energy storage components can reach a charge capacity of 90% SOC (State of Charge) within 15 minutes. The most widely used lithium-ion batteries currently have difficulty meeting the above goals without sacrificing electrochemical performance and safety. Negative electrode materials are considered to be one of the key factors limiting the fast charging capacity of lithium-ion batteries. Non-graphite carbon materials have the advantages of graphite materials as negative electrodes of lithium-ion batteries, and have a wider interlayer spacing and a larger degree of disorder, which is more conducive to the deintercalation of lithium ions. Using non-graphite carbon materials to replace traditional graphite negative electrodes has become an important research and development direction.

[0003] Among non-graphite carbon materials, although hard carbon has advantages such as excellent kinetics, good low-temperature performance, and low tendency to lithium precipitation (lithium precipitation will only occur when it is over-discharged by 120%), its low first coulombic efficiency (< 70%) and high irreversible capacity still limit its large-scale application. Carbon coating is an effective way to solve the low first coulombic efficiency of hard carbon negative electrode, which can reduce the contact area between hard carbon and electrolyte and improve its first coulombic efficiency. At present, carbon coating of hard carbon is usually completed by chemical vapor deposition technology or by mixing and high-temperature carbonization of two types of carbonaceous precursors, which can realize the construction of hard carbon composite materials with core-shell structure (generally speaking, the interior of the core-shell structure is porous hard carbon with high specific surface area, and the outside is a dense carbon layer with low specific surface area), but it has the disadvantages of complex process and high energy consumption; and it is easy to block the pores of the hard carbon in the core during the coating process, increase the diffusion resistance of lithium ions, and reduce the reversible capacity and rate performance of hard carbon. Summary of the invention

[0004] The purpose of the present invention is to provide a hard carbon material with a core-shell structure in order to solve the above technical problems, which can obtain high reversible capacity, high rate performance and high first coulombic efficiency.

[0005] The technical solution of the present invention is a hard carbon material with a core-shell structure, wherein the core is hard carbon with a cross-linked porous structure, and the shell is a dense carbon layer.

[0006] The hard carbon material with a core-shell structure in the present invention has a cross-linked porous structure in the hard carbon core, and the physical structure is relatively stable. The porous structure can provide more lithium ion transmission channels, thereby accelerating the lithium ion transmission rate. The outer shell is a dense carbon layer, which reduces the specific surface area, reduces the lithium ion consumption caused by the contact reaction with the electrolyte, and improves the first coulomb efficiency of the material.

[0007] Furthermore, the hard carbon material I D / I G The (002) interlayer spacing is 0.35-0.38 nm, and the specific surface area is 10-32 m 2 / g, tap density is 0.82~1.1g / cm 3 .

[0008] The present invention also provides a method for preparing the hard carbon material with a core-shell structure, comprising preparing a polyacrylonitrile solution and a sodium alginate solution, mixing the polyacrylonitrile solution and the sodium alginate solution, high temperature treatment, rapid cooling, pre-oxidation treatment and carbonization treatment.

[0009] Further, polyacrylonitrile is dissolved in a non-protonic polar solvent to form a polyacrylonitrile solution with a solid content of 60 to 90 mg / mL.

[0010] Furthermore, the aprotic polar solvent includes, but is not limited to, one or more of dimethyl sulfoxide, acetone, and N,N-dimethylformamide, preferably N,N-dimethylformamide.

[0011] Further, sodium alginate is dissolved in a protic polar solvent to form a sodium alginate solution with a solid content of 20 to 30 mg / mL.

[0012] Furthermore, the protic polar solvent includes, but is not limited to, one or more of deionized water, ethanol, formic acid, and acetic acid, preferably deionized water.

[0013] Furthermore, aprotic polar solvents and protic polar solvents are soluble in each other.

[0014] The present invention uses polyacrylonitrile and sodium alginate as carbonaceous precursors, and uses mutually soluble non-protonic polar solvents and protonic polar solvents as solvents. Due to the different solubility of polyacrylonitrile and sodium alginate in two types of solvents (at room temperature, polyacrylonitrile is soluble in non-protonic polar solvents, and sodium alginate is soluble in protonic polar solvents), a uniform phase will be formed inside the solution during high temperature treatment, and a polyacrylonitrile-rich phase, a sodium alginate-rich phase and a solvent phase will be formed during cooling treatment. After cooling, a gel of polyacrylonitrile-coated sodium alginate is obtained. After the pre-oxidation treatment is initially stabilized for the previous structure, during the carbonization process, sodium alginate has the functions of self-template and self-activation, and a hard carbon core with a cross-linked porous structure and a dense outer shell carbon layer can be formed, thereby realizing the construction of a core-shell structure of a hard carbon material. This method is conducive to achieving good regulation of the morphology and pore structure, and avoids the problem that the current chemical vapor deposition carbon coating technology requires secondary heat treatment of hard carbon and the pores of the hard carbon core are easily blocked.

[0015] Furthermore, when preparing the polyacrylonitrile solution and the sodium alginate solution, the solvents are heated to 80-100°C.

[0016] Furthermore, the volume ratio of the polyacrylonitrile solution to the sodium alginate solution is 15:(3-12).

[0017] Furthermore, the temperature of the high temperature treatment is 80-120°C, and the time is 2-5h; and / or the rapid cooling rate is 5-15°C / min, and the cooling cut-off temperature is 10-12°C.

[0018] Furthermore, after rapid cooling, the obtained gel is soaked in deionized water to dilute and remove the organic solvent inside the gel, thereby preventing the organic solvent from remaining in the carbon material and introducing impurity elements.

[0019] Furthermore, the obtained gel is soaked in deionized water and then dried at 100-120° C. for 10-16 hours.

[0020] Furthermore, the pre-oxidation treatment is carried out at a temperature of 200-250° C. and for a time of 4-6 hours.

[0021] Furthermore, the temperature of the carbonization treatment is 600~1200°C, and the time is 2~4h.

[0022] Furthermore, after the carbonization treatment, the obtained sample is repeatedly washed 3 to 6 times with 0.5 to 1.0 M dilute hydrochloric acid and deionized water, dried at 100 to 120° C. for 10 to 16 hours, and then ball-milled and sieved to obtain a hard carbon material with a core-shell structure.

[0023] The present invention also provides a lithium ion battery negative electrode, comprising the hard carbon material with a core-shell structure.

[0024] Furthermore, the above-mentioned lithium-ion battery negative electrode also includes a conductive agent and a binder.

[0025] Furthermore, the conductive agent is one or more of conductive carbon black, conductive graphite, carbon nanotubes, and carbon fibers.

[0026] Furthermore, the conductive agent is a compound of conductive carbon black and carbon nanotubes in a mass ratio of 1:1-2.

[0027] Furthermore, the binder is one or more of sodium carboxymethyl cellulose, styrene-butadiene rubber, and sodium alginate.

[0028] Furthermore, the binder is a compound of sodium carboxymethyl cellulose and styrene-butadiene rubber in a mass ratio of 1:1-2.

[0029] The method for preparing the negative electrode of the lithium ion battery comprises mixing a hard carbon material with a core-shell structure with a conductive agent and a binder in deionized water, and coating, baking and rolling to prepare the negative electrode of the lithium ion battery.

[0030] Furthermore, the mass percentages of the hard carbon material, the conductive agent, and the binder are 90-95%, 2.0-5.0%, and 3.0-5.0%, respectively.

[0031] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0032] (1) In the present invention, a hard carbon material with a core-shell structure is obtained by phase separation technology, wherein the core is hard carbon with a cross-linked porous structure and the shell is a dense carbon layer, which can obtain high reversible capacity, high rate performance and high first coulombic efficiency;

[0033] (2) The hard carbon core has a cross-linked porous structure with a stable physical structure. The porous structure can provide more lithium ion transmission channels and accelerate the lithium ion transmission rate;

[0034] (3) The dense carbon layer covers the hard carbon material, which has a smaller specific surface area, reduces the lithium ion consumption caused by the contact reaction with the electrolyte, and improves the first coulombic efficiency;

[0035] (4) A polyacrylonitrile-coated sodium alginate gel is formed by phase separation technology, and combined with pre-oxidation and carbonization treatment, a hard carbon core with a cross-linked porous structure and a dense carbon shell are formed to achieve the construction of a core-shell structure of a hard carbon material, which is conducive to achieving good control of the morphology and pore structure;

[0036] (5) The lithium-ion battery negative electrode obtained by the present invention can achieve an initial coulombic efficiency of 92%, a reversible capacity of 560 mAh / g, a capacity retention rate of 96% at high rate, and no capacity decay after 1000 cycles at 1 C;

[0037] (6) The method for preparing the hard carbon material with a core-shell structure in the present invention has a simple process and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a SEM image of the hard carbon material obtained in Example 1;

[0039] Figure 2 This is a SEM image of the hard carbon material obtained in Example 2;

[0040] Figure 3 This is a SEM image of the hard carbon material obtained in Example 3;

[0041] Figure 4 This is the SEM image of the hard carbon material obtained in Example 4. DETAILED DESCRIPTION

[0042] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not used for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosure of the present invention and do not have a limiting effect on the scope of protection. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0043] Example 1

[0044] The preparation method of the hard carbon material with a core-shell structure in this embodiment is as follows:

[0045] (1) Weigh 0.5 g of sodium alginate and add it to 20 mL of deionized water at 85°C and stir for 1 h to obtain a sodium alginate solution; weigh 1.2 g of polyacrylonitrile and add it to 15 mL of N,N-dimethylformamide at 85°C and stir for 1 h to obtain a polyacrylonitrile solution;

[0046] (2) Add 5 mL of sodium alginate solution to 15 mL of polyacrylonitrile solution, stir at 85 °C for 4 h, cool to 10 °C at a cooling rate of 10 °C / min to obtain a gel, soak the gel in deionized water for 24 h, and dry at 80 °C for 12 h to obtain a mixture;

[0047] (3) The mixture was pre-oxidized in an air atmosphere by a tube furnace, heated to 230°C at a heating rate of 5°C / min and kept at that temperature for 6 h. After cooling, the mixture was heated to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere and kept at that temperature for 2 h. After cooling, the product was repeatedly washed three times with deionized water and 0.5 M dilute hydrochloric acid solution, dried at 120°C for 14 h, and subjected to ball milling and screening to obtain a hard carbon material with a core-shell structure (I of the hard carbon material). D / I G is 1.0, the (002) interlayer spacing is 0.365nm, and the specific surface area is 16m 2 / g, tap density is 1.0g / cm 3 ).

[0048] Example 2

[0049] The preparation method of the hard carbon material with a core-shell structure in this embodiment is as follows:

[0050] (1) Weigh 0.6 g of sodium alginate and add it to 20 mL of deionized water at 85°C and stir for 1 h to obtain a sodium alginate solution; weigh 1.3 g of polyacrylonitrile and add it to 15 mL of N,N-dimethylformamide at 85°C and stir for 1 h to obtain a polyacrylonitrile solution;

[0051] (2) Add 5 mL of sodium alginate solution to 15 mL of polyacrylonitrile solution, stir at 100°C for 4 h, cool to 10°C at a cooling rate of 10°C / min to obtain a gel, soak the gel in deionized water for 24 h, and dry at 80°C for 12 h to obtain a mixture;

[0052] (3) The mixture was pre-oxidized in an air atmosphere by a tube furnace, heated to 250°C at a heating rate of 5°C / min and kept at that temperature for 5 h. After cooling, the mixture was heated to 1000°C at a heating rate of 5°C / min in a nitrogen atmosphere and kept at that temperature for 2 h. After cooling, the product was repeatedly washed three times with deionized water and 0.5 M dilute hydrochloric acid solution, dried at 100°C for 16 h, and subjected to ball milling and screening to obtain a hard carbon material with a core-shell structure (I of the hard carbon material). D / I G The (002) interlayer spacing is 0.37 nm and the specific surface area is 26 m 2 / g, tap density is 0.86g / cm 3 ).

[0053] Example 3

[0054] The only difference between this embodiment and embodiment 1 is that in step (2), 10 mL of sodium alginate solution is added to 15 mL of polyacrylonitrile solution.

[0055] Example 4

[0056] The only difference between this embodiment and embodiment 1 is that in step (2), 5 mL of sodium alginate solution is added to 5 mL of polyacrylonitrile solution.

[0057] Example 5

[0058] The only difference between this embodiment and embodiment 1 is that in step (2), 5 mL of sodium alginate solution is added to 30 mL of polyacrylonitrile solution.

[0059] Example 6

[0060] The only difference between this embodiment and embodiment 1 is that the cooling rate of the rapid cooling in step (2) is 2°C / min.

[0061] Example 7

[0062] The only difference between this embodiment and embodiment 1 is that the rapid cooling rate in step (2) is 20° C. / min.

[0063] Comparative Example 1

[0064] The preparation method of the hard carbon material of this comparative example is as follows:

[0065] (1) Weigh 0.5 g of sodium alginate and add it to 20 mL of deionized water at 85°C and stir for 1 h to obtain a sodium alginate solution; weigh 1.2 g of polyacrylonitrile and add it to 15 mL of N,N-dimethylformamide at 85°C and stir for 1 h to obtain a polyacrylonitrile solution;

[0066] (2) Add 5 mL of sodium alginate solution to 15 mL of polyacrylonitrile solution, stir at 85 °C for 4 h, cool to 10 °C at a cooling rate of 10 °C / min to obtain a gel, soak the gel in deionized water for 24 h, and dry at 80 °C for 12 h to obtain a mixture;

[0067] (3) The mixture was heated to 800°C at a heating rate of 5°C / min under a nitrogen atmosphere and kept at this temperature for 8 h. After cooling, the product was repeatedly washed three times with deionized water and 0.5 M dilute hydrochloric acid solution, dried at 120°C for 14 h, and ball-milled and sieved to obtain a hard carbon material.

[0068] Comparative Example 2

[0069] The preparation method of the hard carbon material of this comparative example is as follows:

[0070] (1) Weigh 0.5 g of sodium alginate and 1.2 g of polyacrylonitrile, stir at 85 °C for 1 h, and cool to 10 °C at a cooling rate of 10 °C / min to obtain a mixture;

[0071] (2) The mixture was pre-oxidized in an air atmosphere by heating to 230°C at a heating rate of 5°C / min and kept at that temperature for 6 h. After cooling, the mixture was heated to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere and kept at that temperature for 2 h. After cooling, the mixture was ball-milled and sieved to obtain a hard carbon material.

[0072] Figure 1-3 They are the SEM images of the hard carbon materials obtained in Examples 1-3 respectively. It can be seen that the hard carbon material prepared by the present invention has a core-shell structure, the core has a cross-linked porous structure, and the outer shell is a dense carbon layer. As the amount of sodium alginate increases, the coating effect of the outer shell carbon layer on the inner core porous hard carbon is weakened. Figure 4 It can be seen that when sodium alginate is in excess, a disorderly distributed structure of flake and granular carbon is formed.

[0073] The hard carbon material obtained in the above embodiments and comparative examples is used to prepare a negative electrode for a lithium-ion battery. The specific method includes mixing the hard carbon material with conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose and styrene-butadiene rubber in a mass ratio of 93:1.5:1.5: 2.0:2.0 in deionized water, coating, baking and rolling to prepare the negative electrode for a lithium-ion battery. Commercial lithium-ion battery electrolyte (1M LiPF6in EC / DMC (vol. 1:1)) was used to assemble button cells, and constant current charge and discharge tests were performed. The electrode was metallic lithium and the separator was Celgard 2400. The current density of constant current charge and discharge was 1C=375mA / g, and the voltage range during the test was set to 0.01~3V vs. Li / Li + The physical properties and electrochemical performance data are shown in Table 1.

[0074] Table 1 Physical properties and electrochemical properties data

[0075]

[0076] It can be obtained from the data in Table 1 that when the content of polyacrylonitrile in Example 4 is relatively low, it is difficult to form a core-shell structure, the material has a large specific surface area, and the electrochemical performance is poor. When the content of polyacrylonitrile in Example 5 is relatively high, the thickness of the outer shell carbon layer is relatively thick, the material has a small specific surface area, and the path for lithium ions to migrate into the inner core hard carbon is relatively long, resulting in low reversible capacity and rate performance. When the cooling rate of rapid cooling in Example 6 is too small, the material particle size is relatively large, the coating effect of the outer shell carbon layer is relatively poor, the specific surface area is relatively large, and the first coulomb efficiency is relatively low. When the cooling rate of rapid cooling in Example 7 is too large, the coating effect of the outer shell carbon layer is relatively poor, the specific surface area is relatively large, and the first coulomb efficiency is relatively low. When comparative example 1 is directly carbonized without pre-oxidation, the core-shell structure collapses during the carbonization process, the specific surface area is relatively low, and the reversible capacity and rate performance are relatively low. When comparative example 2 is simply mixed with sodium alginate and polyacrylonitrile without phase separation, it is difficult to form a core-shell structure, the material has a relatively large specific surface area, and the electrochemical performance is relatively poor.

[0077] Finally, it should be noted that the specific embodiments described herein are merely examples of the spirit of the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art of the present invention may make various modifications or supplements to the described embodiments or replace them in similar ways. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A method for preparing a hard carbon material having a core-shell structure, characterized in that: The core of the hard carbon material is hard carbon with a cross-linked porous structure, and the outer shell is a dense carbon layer; The preparation method comprises the steps of preparing a polyacrylonitrile solution and a sodium alginate solution in advance, then mixing the polyacrylonitrile solution and the sodium alginate solution, and finally performing high temperature treatment, rapid cooling, pre-oxidation treatment and carbonization treatment.

2. The preparation method according to claim 1, characterized in that: The hard carbon material I D / I G The (002) interlayer spacing is 0.35-0.38 nm, and the specific surface area is 10-32 m 2 / g, tap density is 0.82~1.1g / cm 3 .

3. The preparation method according to claim 1, characterized in that: Polyacrylonitrile is dissolved in a non-protonic polar solvent to form a polyacrylonitrile solution with a solid content of 60-90 mg / mL.

4. The preparation method according to claim 1, characterized in that: Sodium alginate is dissolved in a proton polar solvent to form a sodium alginate solution with a solid content of 20-30 mg / mL.

5. The preparation method according to claim 1, characterized in that: The volume ratio of polyacrylonitrile solution to sodium alginate solution is 15:(3~12).

6. The preparation method according to claim 1, characterized in that: The temperature of high temperature treatment is 80~120℃ and the time is 2~5h; The cooling rate of rapid cooling is 5~15℃ / min, and the cooling cut-off temperature is 10~12℃.

7. The preparation method according to claim 1, characterized in that: The pre-oxidation treatment is carried out in an air atmosphere at a temperature of 200-250°C for 4-6 hours.

8. The preparation method according to claim 1, characterized in that: The carbonization treatment is carried out in an inert atmosphere at a temperature of 600~1200℃ for 2~4h.

9. A negative electrode for a lithium ion battery, characterized in that: The hard carbon material having a core-shell structure is prepared by the preparation method according to claim 1.

Citation Information

Patent Citations

  • Hard carbon material as well as preparation method and application thereof

    CN113800496A

  • Negative electrode material, negative electrode plate and sodium ion battery

    CN115275191A