Starch-based hard carbon material based on heat-conducting medium as well as preparation method and application of starch-based hard carbon material
Through thermal media treatment and rolling oxidation technology, the foaming and melting problems of starch-based hardcarbon materials in oxidation pretreatment in sodium ion batteries are solved, and high-efficiency and low-cost preparation of starch-based hardcarbon materials are achieved, thereby improving sodium ions Electrochemical properties and reversible capacity of the battery.
Patent Information
- Application Number
- CN202411388176.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The prior art foaming and melting of the oxidation pretreatment process of starch-based hard carbon materials in sodium ion batteries, resulting in increased energy consumption, high cost and difficult to meet the needs of large-scale production, and traditional processes require long-term oxidation cross-linking. Processing limits the application of materials.
Using the preparation method of starch-based hard charcoal material based on heat conduction medium, the heat conduction medium is treated by drying, ball milling or freeze-drying, combined with rolling treatment and multi-stage oxidation-annealing process, avoid foaming and melting, improve oxidation efficiency and material stability, and use water-soluble The thermal conductivity medium of a salt such as sodium chloride, potassium chloride, etc., and the crystal nucleation is inhibited by polyether F-127 to achieve the formation of an ultrafine thermal conductivity medium.
Effectively avoid foaming and melting of starch particles, improve oxidation efficiency and electrochemical performance, simplify the process flow, reduce energy consumption and cost, retain the spherical morphology of starch particles, and significantly improve the reversible ratio of sodium ion batteries. Capacity and first-time Coulomb efficiency.
Smart Images

Figure CN118993033A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a starch-based hard carbon material based on a heat-conducting medium, and a preparation method and application thereof. Background Art
[0002] The growing demand for energy has promoted the development of safe, cheap, scalable and high-performance battery technology. Lithium-ion batteries are difficult to meet the demand due to the limited reserves and uneven distribution of lithium resources. Sodium-ion batteries have similar properties to lithium-ion batteries and show great potential for application. However, Na + Radius Bili + Graphite is a mature commercial negative electrode material for lithium-ion batteries. + It is difficult to intercalate between graphite layers, and the thermodynamic properties of sodium graphite intercalation compounds are unstable. Therefore, it is urgent to develop high-performance negative electrode materials to meet the practical application of sodium-ion batteries.
[0003] Hard carbons (HCs) have the advantages of large interlayer spacing, abundant defects and internal pores, and are the most promising negative electrode materials for sodium ion batteries. Starch, as a widely available biomass material, is abundant in yield and low in cost. It is an ideal precursor for preparing hard carbon materials. In addition, starch itself has a spherical morphology, which can be retained when preparing hard carbon, providing a large number of active sites for the insertion and extraction of sodium ions, which is beneficial to improving the first coulombic efficiency and reversible specific capacity of the battery. However, direct high-temperature carbonization of starch will cause foaming and melting. In order to avoid foaming during starch carbonization, a long-term oxidation cross-linking treatment is required before carbonization. In traditional processes such as air oxidation treatment, the contact between starch particles and air is limited, the oxidation effect is poor, and a longer treatment cycle or higher oxidation temperature is required, resulting in increased energy consumption; in addition, the high-temperature oxidation reaction is violent, which easily leads to starch melting and foaming during oxidation. Liquid phase oxidation is difficult to meet the needs of large-scale production, and often requires additional oxidants, which are difficult to recover, increase the processing steps, and increase production costs. The existing process greatly limits the large-scale production of starch-based hard carbon materials and restricts their application in sodium ion batteries.
[0004] Therefore, it is of great significance to develop a starch oxidation pretreatment and hard carbon-based hard carbon negative electrode material and its preparation method which can maintain the spherical morphology of starch, have high oxidation efficiency, and have a simple and easy treatment method. Summary of the invention
[0005] The purpose of the present invention is to provide a starch-based hard carbon material based on a heat-conducting medium and a preparation method and application thereof in order to overcome the deficiencies of the prior art.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a starch-based hard carbon material based on a heat-conducting medium, comprising the following steps:
[0008] 1) Drying the starch to obtain a carbon precursor;
[0009] Ball milling or freeze drying the heat-conducting medium to obtain a pretreated heat-conducting medium;
[0010] 2) After mixing the carbon precursor and the pretreated heat-conducting medium, pre-oxidation treatment is performed under tumbling conditions, and then the heat-conducting medium and oxidation products are separated;
[0011] 3) The oxidation product is subjected to carbonization and acid washing treatment in sequence under a protective atmosphere to obtain a starch-based hard carbon material;
[0012] Step 1) The heat-conducting medium is a water-soluble salt;
[0013] Step 2) The mass ratio of the carbon precursor to the pretreated heat-conducting medium is 1:1-20.
[0014] Preferably, the starch is potato starch, tapioca starch, pea starch, wheat starch, sorghum starch, rice starch or corn starch.
[0015] Preferably, the drying temperature in step 1) is 30 to 90° C., and the drying time is 2 to 36 hours;
[0016] The heat conducting medium is sodium chloride, potassium chloride, magnesium chloride, sodium carbonate, potassium carbonate or potassium sulfate.
[0017] Preferably, the rotation speed of the ball mill in step 1) is 100-800 r / min, the ball milling time is 1-24 h, and the product is sieved after ball milling, and the sieve mesh number is 100-500 meshes.
[0018] Preferably, a surfactant is added during the freeze-drying process of step 1), wherein the surfactant is a polyether, and the mass ratio of the polyether to the heat-conducting medium is 0.015 to 0.05:1; the freeze-drying temperature is -50 to -40°C, and the freeze-drying time is 6 to 24 hours; and the freeze-drying is followed by sieving with a mesh size of 100 to 600.
[0019] Preferably, in step 2), water is continuously added for pre-oxidation treatment under tumbling conditions, with water added every 25 to 35 minutes, with 4 to 6 mL added each time.
[0020] Preferably, the temperature of the pre-oxidation treatment is 150-400° C., the heating rate is 2-20° C. / min, the time of the pre-oxidation treatment is 1-24 h, and the number of pre-oxidation treatments is 2-6 times.
[0021] Preferably, in step 3), the protective atmosphere is argon or nitrogen, the carbonization temperature is 1100-2600° C., the carbonization time is 1-10 h, and the heating rate to the carbonization temperature is 0.5-20° C. / min.
[0022] The present invention also provides a starch-based hard carbon material based on a heat-conducting medium prepared by the preparation method.
[0023] The present invention also provides the use of the starch-based hard carbon material based on the heat-conducting medium in a sodium ion battery.
[0024] The beneficial effects of the present invention include the following:
[0025] 1) The present invention can effectively physically isolate starch particles and evenly conduct heat by adjusting the size of the heat-conducting medium and replacing heat-conducting medium with different thermal conductivity coefficients, so that starch particles are evenly heated during the oxidation process, avoiding melting and foaming due to excessive local temperature, which is beneficial to the stabilization of starch; in addition, the heat-conducting medium is easy to separate and remove, and hard carbon material can be obtained by taking the precipitate after dissolving it in deionized water, and a reusable heat-conducting medium can be obtained after drying the solution, which has the advantages of simple process, low cost, sustainability and environmental friendliness; the size of the heat-conducting medium can be adjusted by ball milling / freeze drying and screening process, and polyether F-127 is added to freeze-dry the heat-conducting medium. Polyether F-127 inhibits crystal nucleation and growth by increasing the viscosity of the solution and its adsorption on the crystal surface, thereby obtaining an ultrafine heat-conducting medium. Replacing heat-conducting medium with different thermal conductivity coefficients can achieve better oxidation effects.
[0026] 2) The present invention adopts tumbling treatment to fully mix the carbon precursor and the heat-conducting medium, increase the contact between starch particles and oxygen, deepen the degree of oxidation, introduce more electrochemically active oxygen-containing functional groups, and improve the electrochemical performance of the assembled sodium-ion battery; thereby, while ensuring the oxidation effect, the pre-oxidation time is significantly shortened, and the energy consumption and cost in the preparation process are reduced; the heat-conducting medium and tumbling treatment help to conduct heat and improve the starch oxidation efficiency.
[0027] 3) Compared with the single oxidation-annealing treatment, the multi-stage oxidation-annealing treatment of the present invention greatly deepens the degree of oxidation, effectively inhibits the foaming and melting of starch particles that may occur during the carbonization process, retains the natural spherical morphology of starch particles, significantly improves the carbon yield, and has a high reversible capacity and first coulombic efficiency.
[0028] 4) The method of the present invention is simple, environmentally friendly, energy-saving, efficient and feasible. The prepared hard carbon material has a good spherical morphology, providing a large number of active sites for the embedding and extraction of sodium ions. By controlling parameters such as the ratio of carbon precursor and heat conductive medium, oxidation heating rate, oxidation temperature and insulation time, the assembled sodium ion battery can have a higher reversible specific capacity and first coulombic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the preparation method of the starch-based hard carbon material based on the heat-conducting medium of the present invention;
[0030] Figure 2 This is a photo of Example 1 before pre-oxidation treatment;
[0031] Figure 3 This is a photo of Example 1 after pre-oxidation treatment;
[0032] Figure 4 SEM image of the hard carbon material prepared in Example 1;
[0033] Figure 5 SEM image of the hard carbon material prepared for Comparative Example 1;
[0034] Figure 6 SEM image of hard carbon material prepared for Comparative Example 2;
[0035] Figure 7 This is a first cycle charge and discharge curve of the sodium ion button battery assembled in Example 1 at a current density of 20 mA / g. DETAILED DESCRIPTION
[0036] The present invention provides a method for preparing a starch-based hard carbon material based on a heat-conducting medium, comprising the following steps:
[0037] 1) Drying the starch to obtain a carbon precursor;
[0038] Ball milling or freeze drying the heat-conducting medium to obtain a pretreated heat-conducting medium;
[0039] 2) After mixing the carbon precursor and the pretreated heat-conducting medium, pre-oxidation treatment is performed under tumbling conditions, and then the heat-conducting medium and oxidation products are separated;
[0040] 3) The oxidation product is subjected to carbonization and acid washing treatment in sequence under a protective atmosphere to obtain a starch-based hard carbon material;
[0041] Step 1) The heat-conducting medium is a water-soluble salt;
[0042] Step 2) The mass ratio of the carbon precursor to the pretreated heat-conducting medium is 1:1-20.
[0043] In the present invention, the starch is preferably potato starch, tapioca starch, pea starch, wheat starch, sorghum starch, rice starch or corn starch.
[0044] In the present invention, the temperature of the drying treatment in step 1) is preferably 30 to 90° C., more preferably 40 to 80° C., and more preferably 50 to 60° C.; the time of the drying treatment is preferably 2 to 36 h, more preferably 8 to 28 h, and more preferably 10 to 24 h.
[0045] In the present invention, the heat-conducting medium is preferably sodium chloride, potassium chloride, magnesium chloride, sodium carbonate, potassium carbonate or potassium sulfate.
[0046] In the present invention, the rotation speed of the ball mill in step 1) is preferably 100-800 r / min, more preferably 200-600 r / min, and more preferably 300-500 r / min; the ball milling time is preferably 1-24 h, more preferably 5-20 h, and more preferably 8-12 h; after ball milling, the sieve is preferably 100-500 mesh, more preferably 200-400 mesh, and more preferably 300 mesh.
[0047] In the present invention, a surfactant is added during the freeze-drying process of step 1), and the surfactant is preferably a polyether, and the polyether is preferably polyether F-127 (poloxamer, polyoxyethylene polyoxypropylene); the mass ratio of polyether to heat-conducting medium is preferably 0.015 to 0.05:1, more preferably 0.025 to 0.045:1, and more preferably 0.03 to 0.04:1; the temperature of the freeze-drying treatment is preferably -50 to -40°C, more preferably -48 to -42°C, and more preferably -46 to -45°C; the freeze-drying treatment time is preferably 6 to 24h, more preferably 10 to 22h, and more preferably 12 to 20h; after freeze-drying, sieving is performed, and the sieving mesh is preferably 100 to 600 mesh, more preferably 200 to 500 mesh, and more preferably 300 to 400 mesh.
[0048] In the present invention, the mass ratio of the carbon precursor to the pretreated heat-conducting medium in step 2) is preferably 1:2-15, more preferably 1:3-12, and more preferably 1:4-9.
[0049] In step 2) of the present invention, preferably, water is continuously added for pre-oxidation treatment under tumbling treatment conditions, water is added once every 25 to 35 minutes, 4 to 6 mL is added each time, and more preferably, water is added once every 30 minutes, 5 mL is added each time; after pre-oxidation, it is naturally cooled to room temperature.
[0050] In the present invention, the temperature of the pre-oxidation treatment is preferably 150 to 400°C, more preferably 180 to 360°C, and more preferably 200 to 300°C; the heating rate is preferably 2 to 20°C / min, more preferably 5 to 15°C / min, and more preferably 8 to 12°C / min; the time of the pre-oxidation treatment is preferably 1 to 24h, more preferably 3 to 20h, and more preferably 4 to 16h; the number of pre-oxidation treatments is preferably 2 to 6 times, more preferably 3 to 5 times, and more preferably 4 times.
[0051] In the present invention, the separation in step 2) is preferably performed by dissolving the heat-conducting medium and the oxidation product in deionized water and then taking the precipitate to obtain the oxidation product, and drying the solution to obtain a reusable heat-conducting medium.
[0052] In the present invention, the protective atmosphere in step 3) is preferably argon or nitrogen, the carbonization temperature is preferably 1100-2600°C, more preferably 1300-2200°C, and more preferably 1500-20300°C; the carbonization time is preferably 1-10h, more preferably 3-9h, and more preferably 5-8h; the heating rate to the carbonization temperature is preferably 0.5-20°C / min, more preferably 2-15°C / min, and more preferably 5-10°C / min.
[0053] In the present invention, the acid used for the pickling treatment in step 3) is preferably acetic acid solution, hydrochloric acid, sulfuric acid solution or nitric acid solution, and the mass concentration of the acid is preferably 0.5-5%, more preferably 1-4%, and more preferably 2-3%.
[0054] The present invention also provides a starch-based hard carbon material based on a heat-conducting medium prepared by the preparation method.
[0055] The present invention also provides the use of the starch-based hard carbon material based on the heat-conducting medium in a sodium ion battery.
[0056] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0057] Example 1
[0058] 10 g of corn starch was dried in an electric blast drying oven at 60° C. for 10 h to obtain a carbon precursor; 50 g of sodium chloride was ball-milled at a rotation speed of 500 r / min for 4 h, and then sieved using a 500-mesh standard sample sieve to obtain a pretreated heat-conducting medium.
[0059] The carbon precursor was mixed with the pretreated thermal conductive medium, and under tumbling conditions, a trace amount of deionized water was continuously added (5 mL every 30 min) for pre-oxidation treatment; the temperature was increased to 200°C at a heating rate of 5°C / min, kept warm for 1 h, then increased to 240°C at a heating rate of 5°C / min, kept warm for 1 h, then increased to 260°C at a heating rate of 5°C / min, kept warm for 4 h, and naturally cooled to room temperature after pre-oxidation.
[0060] The heat-conducting medium and the oxidation product are dissolved in deionized water, and the precipitate is taken to obtain the oxidation product. The solution is dried to obtain a reusable heat-conducting medium. The oxidation product is carbonized in an argon atmosphere, and the temperature is increased to 800°C at a heating rate of 5°C / min, and then increased to 1400°C at a heating rate of 5°C / min, and kept at 1400°C for 4 hours. After cooling to room temperature, it is pickled with a hydrochloric acid solution with a mass concentration of 2% to obtain a starch-based hard carbon material.
[0061] Starch-based hard carbon material, acetylene black and sodium carboxymethyl cellulose aqueous solution (mass concentration of 2%) are prepared into a slurry in a mass ratio of 92:3:5, coated, dried and cut to obtain electrode sheets, and sodium ion button batteries are assembled using metallic sodium as the counter electrode and 1.0 mol / L NaPF6 solution (the solvent is diethyl carbonate and ethylene carbonate in a volume ratio of 1:1) as the electrolyte.
[0062] The electrochemical performance test of the sodium ion button battery was carried out at a test temperature of 25°C, a current density of 20 mA / g, and a voltage range of 0.001 to 2.5 V. As shown in Table 1, the first cycle charging capacity of the sodium ion button battery assembled in this embodiment is 366.7 mAh / g, and the first coulombic efficiency is 83.9%.
[0063] Example 2
[0064] 10g wheat starch was dried in an electric blast drying oven at 60°C for 8h to obtain a carbon precursor; 2.5g polyether F-127 and 50g sodium chloride were mixed and added to 300mL deionized water, and frozen into a solid at -50°C. The vacuum freeze drying oven was precooled to -50°C, and the obtained frozen solid was placed in a vacuum freeze drying oven for 24h, and then sieved using a 600-mesh standard sample sieve.
[0065] The carbon precursor was mixed with the pretreated thermal conductive medium, and under tumbling conditions, a trace amount of deionized water was continuously added (5 mL every 30 min) for pre-oxidation treatment. The temperature was increased to 220°C at a heating rate of 7°C / min and kept warm for 1.5 h. Then, the temperature was increased to 260°C at a heating rate of 7°C / min and kept warm for 1.5 h. Then, the temperature was increased to 320°C at a heating rate of 7°C / min and kept warm for 6 h. After pre-oxidation, it was naturally cooled to room temperature.
[0066] The heat-conducting medium and the oxidation product are dissolved in deionized water, and the precipitate is taken to obtain the oxidation product. The solution is dried to obtain a reusable heat-conducting medium. The oxidation product is carbonized in an argon atmosphere, and the temperature is increased to 900°C at a heating rate of 6°C / min, and then increased to 1500°C at a heating rate of 3°C / min, and kept at 1500°C for 4 hours. After cooling to room temperature, it is pickled with a sulfuric acid solution with a mass concentration of 3% to obtain a starch-based hard carbon material.
[0067] Starch-based hard carbon material, acetylene black and sodium carboxymethyl cellulose aqueous solution (mass concentration of 2%) are prepared into a slurry in a mass ratio of 92:3:5, and the slurry is coated, dried and cut to obtain electrode sheets. Sodium ion button batteries are assembled using metallic sodium as the counter electrode and 1.0 mol / L NaPF6 solution (the solvent is diethyl carbonate and ethylene carbonate in a volume ratio of 1:1) as the electrolyte.
[0068] The electrochemical performance test of the sodium ion button battery was carried out at a test temperature of 25°C, a current density of 20 mA / g, and a voltage range of 0.001 to 2.5 V. As shown in Table 1, the first cycle charging capacity of the sodium ion button battery assembled in this embodiment is 353.4 mAh / g, and the first coulombic efficiency is 85.2%.
[0069] Example 3
[0070] 10g corn starch was dried in an electric blast drying oven at 65°C for 10h to obtain a carbon precursor; 2.1g polyether F-127 and 70g potassium chloride were mixed and added to 300mL deionized water, and frozen into a solid at -40°C. The vacuum freeze drying oven was precooled to -40°C, and the obtained frozen solid was placed in a vacuum freeze drying cabinet for 12h, and then sieved using a 500-mesh standard sample sieve.
[0071] The carbon precursor was mixed with the pretreated thermal conductive medium, and under tumbling conditions, a trace amount of deionized water was continuously added (5 mL every 30 min) for pre-oxidation treatment. The temperature was increased to 190°C at a heating rate of 10°C / min and kept for 1 h. Then, the temperature was increased to 210°C at a heating rate of 10°C / min and kept for 1 h. Then, the temperature was increased to 250°C at a heating rate of 10°C / min and kept for 3 h. After pre-oxidation, it was naturally cooled to room temperature.
[0072] The heat-conducting medium and the oxidation product are dissolved in deionized water, and the precipitate is taken to obtain the oxidation product. The solution is dried to obtain a reusable heat-conducting medium. The oxidation product is carbonized in an argon atmosphere, and the temperature is increased to 700°C at a heating rate of 4°C / min, and then increased to 1300°C at a heating rate of 1°C / min, and kept at 1300°C for 8 hours. After cooling to room temperature, it is pickled with a sulfuric acid solution with a mass concentration of 1% to obtain a starch-based hard carbon material.
[0073] Starch-based hard carbon material, acetylene black and sodium carboxymethyl cellulose aqueous solution (mass concentration of 2%) are prepared into a slurry in a mass ratio of 92:3:5, and the slurry is coated, dried and cut to obtain electrode sheets. Sodium ion button batteries are assembled using metallic sodium as the counter electrode and 1.0 mol / L NaPF6 solution (the solvent is diethyl carbonate and ethylene carbonate in a volume ratio of 1:1) as the electrolyte.
[0074] The electrochemical performance test of the sodium ion button battery was carried out at a test temperature of 25°C, a current density of 20 mA / g, and a voltage range of 0.001 to 2.5 V. As shown in Table 1, the first cycle charging capacity of the sodium ion button battery assembled in this embodiment is 362.9 mAh / g, and the first coulombic efficiency is 82.6%.
[0075] Example 4
[0076] 10 g of corn starch was dried in an electric blast drying oven at 70° C. for 6 h to obtain a carbon precursor; 60 g of magnesium chloride was ball-milled at a rotation speed of 200 r / min for 16 h, and then sieved using a 400-mesh standard sample sieve.
[0077] The carbon precursor was mixed with the pretreated thermal conductive medium, and under tumbling conditions, a trace amount of deionized water was continuously added (5 mL every 30 min) for pre-oxidation treatment. The temperature was increased to 210°C at a heating rate of 6°C / min and kept warm for 1.5 h. Then, the temperature was increased to 250°C at a heating rate of 6°C / min and kept warm for 1.5 h. Then, the temperature was increased to 290°C at a heating rate of 6°C / min and kept warm for 6 h. After pre-oxidation, it was naturally cooled to room temperature.
[0078] The heat-conducting medium and the oxidation product are dissolved in deionized water, and the precipitate is taken to obtain the oxidation product. The solution is dried to obtain a reusable heat-conducting medium. The oxidation product is carbonized in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 3°C / min, and then increased to 1600°C at a heating rate of 3°C / min, and kept at 1600°C for 4 hours. After cooling to room temperature, it is pickled with a sulfuric acid solution with a mass concentration of 3% to obtain a starch-based hard carbon material.
[0079] Starch-based hard carbon material, acetylene black and sodium carboxymethyl cellulose aqueous solution (mass concentration of 2%) are prepared into a slurry in a mass ratio of 92:3:5, and the slurry is coated, dried and cut to obtain electrode sheets. Sodium ion button batteries are assembled using metallic sodium as the counter electrode and 1.0 mol / L NaPF6 solution (the solvent is diethyl carbonate and ethylene carbonate in a volume ratio of 1:1) as the electrolyte.
[0080] The electrochemical performance test of the sodium ion button battery was carried out at a test temperature of 25°C, a current density of 20 mA / g, and a voltage range of 0.001 to 2.5 V. As shown in Table 1, the first cycle charging capacity of the sodium ion button battery assembled in this embodiment is 342.2 mAh / g, and the first coulombic efficiency is 87.7%.
[0081] Comparative Example 1
[0082] No pre-oxidation treatment was used, and direct carbonization was performed. Other conditions were the same as those in Example 1.
[0083] Comparative Example 2
[0084] No heat-conducting medium was added, and other conditions were the same as those in Example 1.
[0085] Comparative Example 3
[0086] The tumbling process is not adopted, and other conditions are the same as those in Example 1.
[0087] Comparative Example 4
[0088] The mass of the heat conducting medium was changed to 20 g, and other conditions were the same as those in Example 1.
[0089] The reversible capacity and first coulombic efficiency of the assembled sodium ion button cells of the embodiment and the comparative example are shown in Table 1.
[0090] Table 1 Reversible capacity and first coulombic efficiency of assembled sodium ion button cells of Examples and Comparative Examples
[0091] Reversible capacity (mAh / g) First coulombic efficiency / % Example 1 366.7 83.9 Example 2 353.4 85.2 Example 3 362.9 82.6 Example 4 342.2 87.7 Comparative Example 1 185.3 60.5 Comparative Example 2 216.4 63.8 Comparative Example 3 247.4 71.3 Comparative Example 4 234.6 68.9
[0092] It can be seen from Example 1 and Comparative Example 1 that the pre-oxidation treatment before carbonization is beneficial to the stabilization of starch particles. The prepared hard carbon material can retain the original spherical morphology of the carbon precursor, providing a large number of active sites for the embedding and extraction of sodium ions, which is beneficial to improving the reversible capacity and the first coulombic efficiency.
[0093] It can be seen from Example 1 and Comparative Example 2 that the addition of a heat-conducting medium can effectively physically isolate starch particles, evenly conduct heat, and avoid melting and foaming due to excessive local temperature.
[0094] It can be seen from Example 1 and Comparative Example 3 that the tumbling process can make the starch particles heat evenly during the pre-oxidation process, which is beneficial to increase the contact between starch and oxygen and improve the oxidation efficiency.
[0095] It can be seen from Example 1 and Comparative Example 4 that less heat-conducting medium will affect the effect of heat conduction, thereby affecting the spherical morphology of the hard carbon material and the final electrochemical performance.
[0096] In addition, it can be seen from Examples 1 to 4 that parameters such as the type of carbon precursor, pre-oxidation heating rate, pre-oxidation temperature and holding time, number of pre-oxidation times, carbonization heating rate, carbonization temperature and holding time, pickling type and concentration will also affect the electrochemical properties of the assembled sodium ion battery.
[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing starch-based hard carbon material based on a heat-conducting medium, characterized in that: The following steps are included: 1) Drying the starch to obtain a carbon precursor; Ball milling or freeze drying the heat-conducting medium to obtain a pretreated heat-conducting medium; 2) After mixing the carbon precursor and the pretreated heat-conducting medium, pre-oxidation treatment is performed under tumbling conditions, and then the heat-conducting medium and oxidation products are separated; 3) The oxidation product is subjected to carbonization and acid washing treatment in sequence under a protective atmosphere to obtain a starch-based hard carbon material; Step 1) The heat-conducting medium is a water-soluble salt; Step 2) The mass ratio of the carbon precursor to the pretreated heat-conducting medium is 1:1-20.
2. The preparation method according to claim 1, characterized in that: The starch is potato starch, tapioca starch, pea starch, wheat starch, sorghum starch, rice starch or corn starch.
3. The preparation method according to claim 2, characterized in that: Step 1) The drying temperature is 30 to 90° C. and the drying time is 2 to 36 hours; The heat conducting medium is sodium chloride, potassium chloride, magnesium chloride, sodium carbonate, potassium carbonate or potassium sulfate.
4. The preparation method according to claim 3, characterized in that: Step 1) The rotation speed of the ball mill is 100-800 r / min, the ball milling time is 1-24 h, and the product is sieved after ball milling, and the sieve mesh number is 100-500 meshes.
5. The preparation method according to claim 3, characterized in that: Step 1) During the freeze-drying process, a surfactant is added, wherein the surfactant is a polyether, and the mass ratio of the polyether to the heat-conducting medium is 0.015 to 0.05:1; the freeze-drying temperature is -50 to -40°C, and the freeze-drying time is 6 to 24 hours; after the freeze-drying, the product is sieved with a mesh size of 100 to 600.
6. The preparation method according to claim 4 or 5, characterized in that: In step 2), water is continuously added for pre-oxidation treatment under tumbling conditions, with water added every 25 to 35 minutes, with 4 to 6 mL added each time.
7. The preparation method according to claim 6, characterized in that: The temperature of the pre-oxidation treatment is 150-400° C., the heating rate is 2-20° C. / min, the time of the pre-oxidation treatment is 1-24 hours, and the number of pre-oxidation treatments is 2-6 times.
8. The preparation method according to claim 7, characterized in that: Step 3) The protective atmosphere is argon or nitrogen, the carbonization temperature is 1100-2600°C, the carbonization time is 1-10h, and the heating rate to the carbonization temperature is 0.5-20°C / min.
9. Starch-based hard carbon material based on a heat-conducting medium prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the starch-based hard carbon material based on a heat-conducting medium as claimed in claim 9 in a sodium ion battery.
Citation Information
Patent Citations
Preparation method of spherical carbon anode material for lithium ion battery
CN107706417A
Preparation method of mono-dispersed nano particle material
CN112250043A
Preparation method of sodium ion battery negative electrode material
CN113620272A
Sulfur-doped biomass hard carbon material as well as preparation method and application thereof
CN113912039A
Composite carbon microspheres as well as preparation method and application thereof
CN114873579A
Cited By
High-tap-density hard carbon material as well as preparation method and application thereof
CN122166753A