Quick-filling type coal-based graphite material as well as preparation method and application thereof
Through physical sorting and high-temperature graphitization processes, high-performance coal-based graphite materials were prepared, solving the problems of limited graphite resources and complex processes in the existing technology, and achieving high capacity, long cycle life and low cost lithium-ion battery negative electrodes Material.
Patent Information
- Application Number
- CN202411119990.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
The graphite resources of the negative electrode material of existing lithium-ion batteries are limited, the preparation process is complex, the raw material cost is high, and the coal rock components of different properties in the coal are not fully utilized, resulting in low carbon yield and poor cycle stability, which is unable to meet high-performance storage. Can demand.
Coal powder with suitable particle size and inert group content was obtained through physical sorting, and was pickled and dried, followed by graphitization in a high-temperature graphitization furnace to prepare coal-based graphite materials with high specific capacity and high rate performance. .
It has achieved a high order and high lithium storage electrochemical performance of coal-based graphite materials, improved the transmission and storage capacity of lithium ions, significantly improved the charging capacity and cycle stability of lithium ion batteries, and met industrial needs.
Smart Images

Figure CN118993056A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a fast-charging coal-based graphite material. Background Art
[0002] The energy crisis and environmental problems caused by the excessive consumption of traditional fossil fuels urgently require people to develop and efficiently utilize renewable clean new energy. In recent years, with the rapid development of new energy vehicles and multifunctional electronic products, the development and application of lithium-ion batteries have become increasingly important. At present, the commercially mature negative electrode material of lithium-ion batteries is still the graphite negative electrode. However, natural graphite resources are limited, and it is difficult to separate and purify, has poor rate performance, and poor cycle stability, which cannot meet the market demand for high-performance energy storage. However, natural graphite resources are limited, and it is of great practical significance to find a high-carbon raw material with a wide source and low cost for the preparation of artificial graphite materials. Coal is a complex three-dimensional cross-linked structure with an aromatic structure as a skeleton and an alkyl chain structure as a filler. It is low in price and is one of the preferred materials for synthesizing artificial graphite materials.
[0003] At present, the raw materials for preparing coal-based graphite are mainly coal-based needle coke and oil-based needle coke, which generally have problems such as low carbon yield, high raw material price and low tap density of coal-based graphite. Coal is the carbon source with the highest carbon yield and the lowest raw material price. However, my country has all kinds of coal from lignite to anthracite, but the degree of coal metamorphism in different regions is different, and the coal properties of the same coal in different regions are also different, which leads to difficulties in the selection of raw coal and direct material utilization. In recent years, researchers have used coal-based materials for secondary modification to improve electrochemical performance. For example, patent CN109768217A discloses a method for preparing graphite materials, including mixing needle coke preparation raw materials with aromatic heterocyclic compounds for co-carbonization, and then preparing graphite materials through graphitization treatment. Since the S / N in the heterocyclic ring is removed in the subsequent treatment, leaving ion channels, and the subsequent modifier coating treatment, it is convenient for subsequent lithium ion diffusion and improves the rate performance of graphite materials, but its process is relatively complicated and the raw material cost is high. CN103346294B discloses a method for preparing an artificial graphite negative electrode material, which first coats the ultrafine powdered coating material and the crushed and spheroidized artificial graphite in a mechanical fusion machine, and then performs roasting and graphitization to obtain the artificial graphite negative electrode material. The invention can improve the rate performance of the negative electrode material, but due to the use of a large amount of asphalt, a soft carbon intercalation is formed, which reduces the capacity of the negative electrode material. CN115472827A discloses a coal-based graphite negative electrode material and its preparation method and application, which first selects coal samples with a vitrinite reflectance of >2, volatile matter <10wt%, and ash content <10wt% after grinding, and performs carbonization and graphitization to prepare coal-based graphite with high discharge capacity, but it has high requirements for raw coal, and no physical sorting and enrichment are performed, resulting in a low yield of coal samples that meet the requirements. However, the above scheme uses coal as a raw material with uniform properties to directly prepare graphite materials, ignoring the difference in reflectivity caused by coal rock components with different properties in coal, and failing to fully utilize the properties of raw coal, resulting in a complex process flow. Therefore, developing a process for enriching specific coal rock components in coal to obtain a method for preparing high-performance coal-based graphite materials from coal rock components is the key to achieving widespread application of coal-based carbon materials in the field of energy storage. Summary of the invention
[0004] One of the purposes of the present invention is to invent a method for preparing a fast-filling coal-based graphite material, using coal, which is abundant in reserves and low in cost, as a carbon source for preparing the graphite material.
[0005] The second object of the present invention is to provide a coal-based graphite material prepared by the above preparation method, which has high specific capacity, high rate performance and cycle stability.
[0006] The third object of the present invention is to provide the application of the above-mentioned coal-based graphite material as a negative electrode material for lithium-ion batteries.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing a fast-filling coal-based graphite material, comprising the following steps:
[0009] (1) crushing and screening the raw coal to obtain coal powder with a particle size ranging from 0.5 to 3.0 mm;
[0010] (2) physically sorting the coal powder obtained in step (1), and drying the resulting coal powder to obtain a sorted coal sample having an inert group content of 30 to 66%;
[0011] (3) performing secondary crushing and screening on the selected coal sample obtained in step (2) to obtain coal powder with a particle size of less than 0.074 mm;
[0012] (4) acid-washing the coal powder obtained in step (3), washing with water until neutral, and drying to obtain an ultrapure coal sample with an ash content of less than 0.5 wt %;
[0013] (5) The ultrapure coal sample obtained in step (4) is placed in a graphite crucible of a high-temperature graphitization furnace, and graphitized under a slightly positive pressure of 20-30 kPa and an inert atmosphere to obtain a coal-based graphite material.
[0014] Preferably, the D90 particle size of the coal powder in step (1) is 0.5-1.0 mm.
[0015] Preferably, the raw coal in step (1) is selected from one or more of anthracite, lean coal, lean coal, coking coal, fat coal, gas coal, slightly sticky coal, non-sticky coal and long flame coal.
[0016] Preferably, the D50 particle size of the coal powder in step (3) is 0.005-0.020 mm.
[0017] Preferably, the acid used for pickling in step (4) is a medium-strong acid, more preferably at least one of hydrochloric acid, nitric acid, hydrofluoric acid and sulfuric acid.
[0018] Preferably, the graphitization temperature in step (5) is 2500-3000° C.; the heating rate is 1-10° C. / min; and the insulation time is 1-6 h.
[0019] Preferably, the inert atmosphere in step (5) comprises one of nitrogen, helium, argon, neon and xenon.
[0020] In a second aspect, the present invention provides a coal-based graphite material prepared by the above preparation method.
[0021] The coal-based hard carbon material 002The interlayer spacing is 0.3373-0.3382nm, the first charge capacity is 280-365mAh / g at a current density of 0.1C, and the average charge capacity is >100mAh / g at a current density of 5C, showing excellent lithium-ion battery performance. 002 The interlayer spacing is within a suitable range (0.3373-0.3377 nm), the first charge capacity is >340 mAh / g, and the charge capacity at 5C current density is >190 mAh / g.
[0022] In a third aspect, the present invention provides the use of the above-mentioned coal-based graphite material as a negative electrode material for lithium-ion batteries.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The method for preparing coal-based graphite material provided by the present invention has the advantages of low raw material cost, simple preparation process and high carbon yield. It utilizes coal rock components with different properties contained in coal, and increases the content of inert groups in coal through physical separation while reducing the mineral content in coal. It adjusts the molecular configuration of graphite precursor, combines a one-step high-temperature graphitization process, reduces the mass loss of coal during the heating process, and obtains graphite microcrystals with high order and higher lithium storage electrochemical performance, which is beneficial to the transmission and storage of lithium ions.
[0025] 2. The graphite material prepared by the present invention has a suitable d 002 The interlayer spacing and larger lithium storage capacity, as a lithium battery negative electrode material, it has high reversible capacity (>350mAh / g), excellent rate performance (2C / 0.1C>80%, 5C reversible capacity>200mAh / g) and cycle stability (cycle number greater than 800), showing excellent lithium ion battery fast charging performance. The present invention provides a coal-based graphite material with high energy density, long cycle life, excellent rate performance and low cost, which can well meet the needs of industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Characteristic diagram of microscopic components of coal samples after sorting in step (2) of Example 1 and Comparative Example 1 under an optical microscope;
[0027] Figure 2 Transmission electron microscopy (TEM) of the coal-based graphite materials prepared in Example 1 and Comparative Example 1;
[0028] Figure 3 X-ray diffraction patterns (XRD) of coal-based graphite materials prepared in Example 1 and Comparative Example 1;
[0029] Figure 4 The charge and discharge curves of the coal-based lithium-ion batteries prepared in Example 1 and Comparative Example 1;
[0030] Figure 5 The coal-based lithium-ion battery rate characteristic curves prepared in Example 1 and Comparative Example 1;
[0031] Figure 6 This is the long cycle diagram of the coal-based lithium-ion battery prepared in Example 1. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0033] Example 1
[0034] This embodiment provides a method for preparing a fast-filling coal-based graphite material, comprising the following steps:
[0035] (1) putting the coking coal into a 1 mm sieve for sieving, and then putting the undersize material into a 0.5 mm sieve for sieving to obtain the oversize material;
[0036] (2) Weigh 1 kg of the coal sample obtained in step (1) and pour it into a mesh bucket. Wash the coal slime attached to the coal blocks with water, filter out the washing water and put it into a heavy liquid with a density of 1.35 kg / L prepared with ZnCl2 as a floating and sinking medium. Slowly move the mesh bucket up and down, then let it stand for 3 to 5 minutes to separate the layers, remove all the floating objects on the upper layer, lift the mesh bucket containing the sinking objects, filter out all the heavy liquid, and then put it into the heavy liquid with a density of 1.40 kg / L. Repeat the above steps to obtain a coal sample with a density of 1.35 to 1.40 kg / L. Rinse the residual zinc chloride on the product with hot water, then put it into a drying oven at a temperature of 80°C to dry. After drying, take it out and cool it to obtain a coal sample with an inert group content of about 65%;
[0037] (3) Grinding the sorted coal sample obtained in step (2) into powder with a mesh size of less than 200, and sieving the sieved material to obtain fine coal powder;
[0038] (4) 50 g of the fine powder obtained in step (3) was placed in a mixture of 50 mL of hydrochloric acid (5 mol / L), the mixture was stirred at 70° C. for 12 h, and washed with deionized water until the pH value was about 7;
[0039] (5) Dry the sample obtained in step (3) in an oven at 60° C. for 8 hours, and then repeat the above operation with HF (40%\22.6 mol / L);
[0040] (6) The sample is placed in a high-temperature graphitization furnace using a graphite crucible, and the temperature is raised to 2800°C at a rate of 10°C / min in high-purity argon gas under a slightly positive pressure (20-30 kPa), and kept warm for 3 hours. After the sample is naturally cooled to room temperature, a coal-based graphite material is obtained.
[0041] Example 2
[0042] The difference between this embodiment and embodiment 1 is that: in step (2), 1 kg of coal sample is weighed and poured into a net bottom bucket, the coal slime attached to the coal block is washed with water, the washing water is filtered out and then put into a heavy liquid with a density of 1.30 kg / L prepared with ZnCl2 as a floating and sinking medium, the net bottom bucket is slowly moved up and down, and then it is allowed to stand for 3 to 5 minutes to separate the layers, the upper floating objects are scooped out, the net bottom bucket containing the sinking objects is lifted up and the heavy liquid is filtered out, and then put into the heavy liquid with a density of 1.35 kg / L, and the above steps are repeated, the zinc chloride remaining on the product is washed off with hot water, and then it is dried in a drying oven at a temperature not higher than 80°C to obtain a coal sample with an inert group content of about 31%. The other steps and parameters are the same as those in embodiment 1.
[0043] Example 3
[0044] The difference between this embodiment and embodiment 1 is that in step (7), the sample is placed in a high-temperature graphitization furnace using a graphite crucible, and the temperature is raised to 2600° C. at 10° C. / min in a high-purity argon atmosphere, and the temperature is kept for 3 hours. After the sample is naturally cooled to room temperature, a coal-based graphite material is obtained. The other steps and parameters are the same as those in embodiment 1.
[0045] Example 4
[0046] The difference between this embodiment and embodiment 2 is that: in step (7), the sample is placed in a high-temperature graphitization furnace using a graphite crucible, and the temperature is raised to 2600° C. at 10° C. / min in a high-purity argon atmosphere, and the temperature is kept for 3 hours. After the sample is naturally cooled to room temperature, a coal-based graphite material is obtained. The other steps and parameters are the same as those in embodiment 1.
[0047] Comparative Example 1
[0048] The difference between this comparative example and Example 1 is that: in step (2), 1 kg of coal sample is weighed and poured into a net bottom bucket, the coal slime attached to the coal block is washed with water, the washing water is filtered out and then put into a heavy liquid with a density of 1.30 kg / L prepared with ZnCl2 as a floating and sinking medium, the net bottom bucket is slowly moved up and down, and then it is allowed to stand for 3 to 5 minutes to separate the layers, the upper floating objects are removed, and then it is placed in a drying oven at a temperature of 80°C for drying, and after drying, it is taken out and cooled to obtain a coal sample with an inert group content of about 11%. The other steps and parameters are the same as those in Example 1.
[0049] See also Figure 1 , Figure 1 The characteristic diagram of the microscopic components of the coal sample of Example 1 and Comparative Example 1 under an optical microscope. The left figure is the coal sample after sorting in step (2) of Example 1, and the right figure is the coal sample after sorting in step (2) of Comparative Example 1.
[0050] Depend on Figure 1It can be seen that the inert content in coal samples separated by heavy liquids of different densities is significantly different, and the higher the density of the separation heavy liquid, the more inert content in the coal.
[0051] See also Figure 2 , Figure 2 The transmission electron microscope (TEM) images of the coal-based hard carbon materials prepared in Example 1 and Comparative Example 1 are shown in FIG.
[0052] By comparing the transmission electron microscope (TEM) images of coal-based graphite materials prepared with an inert group content of about 65% and an inert group content of about 11%, it can be seen that the increase in the inert group content in coal is conducive to the development of the graphite microcrystalline structure and the formation of a long-range ordered carbon network structure.
[0053] See also Figure 3 , Figure 3 The X-ray diffraction (XRD) diagrams of the coal-based graphite materials prepared in Example 1 and Comparative Example 1 are shown. The upper curve is the coal-based graphite material prepared in Example 1, and the lower curve is the coal-based graphite material prepared in Comparative Example 1.
[0054] Depend on Figure 3 It can be seen that the effect of inert group content in different coals on the interlayer spacing (d 002 ) is the influence of the interlayer spacing (d 002 ) decreased from 0.3382nm to 0.3373nm, indicating that the interlayer spacing (d 002 ) is small, the degree of graphitization is high, and there are sufficient lithium storage sites.
[0055] Comparative Example 2
[0056] The difference between this comparative example and Example 3 is that: in step (2), 1 kg of coal sample is weighed and poured into a net bottom bucket, the coal slime attached to the coal block is washed with water, the washing water is filtered out and then put into a heavy liquid with a density of 1.30 kg / L prepared with ZnCl2 as a floating and sinking medium, the net bottom bucket is slowly moved up and down, and then it is allowed to stand for 3 to 5 minutes to separate the layers, the upper floating objects are removed, and then it is placed in a drying oven at a temperature of 80°C for drying, and after drying, it is taken out and cooled to obtain a coal sample with an inert group content of about 11%. The other steps and parameters are the same as those in Example 1.
[0057] Comparative Example 3
[0058] The difference between this embodiment and embodiment 1 is that the raw coking coal is directly deashed after crushing and screening, without the physical separation process in step (2), wherein the vitrinite content of the raw coking coal is about 75%. The other steps and parameters are the same as those in embodiment 1.
[0059] Battery assembly and testing
[0060] The coal-based graphite material for the negative electrode of the lithium-ion battery prepared above was mixed with carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1, and then the slurry was coated on the carbon-coated copper foil. After drying at 70°C, a 10mm electrode sheet was made by a slicer, and the electrode sheet was dried at 80°C for 5h under vacuum. A metal lithium sheet was used as the negative electrode, and the electrode sheet of the embodiment and the comparative example was used as the positive electrode. 1mol / L lithium hexafluorophosphate (LiPF6) was mixed with ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1, and 5% fluoroethylene carbonate (FEC) was added as the electrolyte, and a CR2025 button cell was assembled in a glove box. A high-precision battery tester (Wuhan Blue Electric) was used to perform constant current charge and discharge tests at a current density of 0.1C (1C = 350mA / g) and a voltage range of 0-3.0V. The test results are shown in Table 1.
[0061] Table 1
[0062]
[0063]
[0064] It can be seen from the specific surface data in Table 1 that the inert group content of coal-based graphite material has a certain influence on the interlayer spacing of coal-based graphite. When the inert group content is the same, the increase in graphitization temperature helps to improve the charging capacity, such as Example 1, Example 2 and Comparative Example 1 and Comparative Example 2, and the charging capacity is 355.85mAh / g, 296.71mAh / g, 201.40mAh / g and 281.81mAh / g respectively. The reason is that the high temperature of 2800°C promotes the development of graphite crystallites, reduces graphite defects, and reduces the lithium ion transmission resistance in the negative electrode material. When the content of inertin group in coal increases, such as in Example 1 and Example 1, the first charging capacity is 355.85 mAh / g and 296.71 mAh / g respectively. The reason is that the vitrinite in coal produces a large amount of volatiles during high-temperature pyrolysis, which easily forms chaotic graphite. The inertinite has lower reaction activity than other coal rock components in the high-temperature process and easily produces highly ordered graphite, so that its interlayer spacing reaches 0.3373 nm, which is close to the theoretical graphite interlayer spacing. Therefore, the inertinite content of coal-based graphite material is within a suitable range (30-70%), which is easy to form highly ordered graphite.
[0065] Figure 4 The charge and discharge curves of the coal-based lithium-ion battery prepared in Example 1 and Comparative Example 1 are shown in FIG. Figure 4It can be seen that the comparison of the withholding test data of coal-based graphite materials shows the impact on the lithium storage performance of coal-based graphite negative electrode materials. Since the graphite micro-sheet layers of coal-based graphite are relatively complete and directionally stacked to form highly ordered three-dimensional graphite microcrystals, the first charging capacity is increased to 355.85mAh / g at a current density of 0.1C.
[0066] Figure 5 The coal-based lithium-ion battery rate characteristic curves prepared in Example 1 and Comparative Example 1 are shown in FIG. Figure 5 It can be seen that under different current densities, since the coal-based graphite in Example 1 has a graphite interlayer spacing that is more suitable for rapid lithium insertion / delithiation, and the graphite microchip layers are stacked in a more orderly manner, the diffusion resistance of lithium ions between graphite layers is reduced, so that when the current density increases from 0.1C to 2C, the graphite negative electrode in Example 1 still has a capacity retention rate of 80%, and has a reversible capacity of 201.33 mAh / g at a high current density (5C).
[0067] Figure 6 This is a long cycle diagram of the coal-based lithium-ion battery prepared in Example 1. Figure 6 It can be seen that at a current density of 1C, after 850 cycles, its capacity retention rate is close to 100%, showing good long-cycle performance.
[0068] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a fast-filling coal-based graphite material, It is characterized in that The following steps are involved: (1) crushing and screening the raw coal to obtain coal powder with a particle size ranging from 0.5 to 3.0 mm; (2) physically sorting the coal powder obtained in step (1), and drying the resulting coal powder to obtain a sorted coal sample having an inert group content of 30 to 66%; (3) performing secondary crushing and screening on the selected coal sample obtained in step (2) to obtain coal powder with a particle size of less than 0.074 mm; (4) acid-washing the coal powder obtained in step (3), washing with water until neutral, and drying to obtain an ultrapure coal sample with an ash content of less than 0.5 wt %; (5) The ultrapure coal sample obtained in step (4) is placed in a graphite crucible of a high-temperature graphitization furnace, and graphitized under a slightly positive pressure of 20-30 kPa and an inert atmosphere to obtain a coal-based graphite material.
2. A method for preparing a fast-filling coal-based graphite material according to claim 1, It is characterized in that The D90 particle size of the coal powder in step (1) is 0.5-1.0 mm.
3. A method for preparing a fast-filling coal-based graphite material according to claim 1, It is characterized in that The raw coal in step (1) is selected from one or more of anthracite, lean coal, lean coal, coking coal, fat coal, gas coal, slightly sticky coal, non-sticky coal and long flame coal.
4. A method for preparing a fast-filling coal-based graphite material according to claim 1, It is characterized in that The physical separation in step (2) includes a method selected from the group consisting of hand separation, flotation, gravity separation, centrifugation, and electrostatic separation.
5. A method for preparing a fast-filling coal-based graphite material according to claim 1, It is characterized in that The acid used for pickling in step (4) is selected from at least one of hydrochloric acid, nitric acid, hydrofluoric acid and sulfuric acid.
6. A method for preparing a fast-filling coal-based graphite material according to claim 1, It is characterized in that The graphitization temperature in step (5) is 2500-3000° C., the heating rate is 1-10° C. / min, and the insulation time is 1-6 h.
7. A method for preparing a fast-filling coal-based graphite material according to claim 1, It is characterized in that The inert atmosphere in step (5) includes one of nitrogen, helium, argon, neon and xenon.
8. A coal-based graphite material obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the coal-based graphite material according to claim 8 as a negative electrode material for lithium-ion batteries.
Citation Information
Patent Citations
Method for preparing graphene with anthracite as raw material
CN105502364A
Process for preparing ultra-pure coal by using acid-alkali method
CN112662446A
Graphite negative electrode material and preparation method and application thereof
CN115472830A
Coal-based hard carbon material as well as preparation method and application thereof
CN117401669A
Selection and preparation method of feed coal for preparing coal-based carbon negative electrode material
CN117849149A
Cited By
Method for preparing lithium battery negative electrode material from anthracite and application of lithium battery negative electrode material
CN122586025A