Joint body, ceramic circuit substrate and semiconductor device using the same
By optimizing the Ag distribution of the bonding layer of the ceramic circuit substrate, the problem of inconsistent etching effects in the active metal bonding method is solved, more stable etching and bonding strength are achieved, and the dimensional deviation of the bonded body is reduced.
Patent Information
- Application Number
- CN202180055457.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-10-19
AI Technical Summary
In the bonding layer formed by the active metal bonding method, in the structure where Ag and Cu are mixed, the removal effect of the etching liquid varies, resulting in variations in the size of the protrusions of the bonding layer.
By controlling the Ag distribution in the joint layer to ensure that the area ratio of the Ag-rich region is less than 70% in the measurement area in the thickness direction and orthogonal direction, the thickness and composition of the joint layer are optimized to improve etching and joint strength.
It effectively reduces the area of the difficult-to-etch area during the etching process, improves the etching performance and joint strength of the joint body, reduces the deviation in the size of the protrusion, and improves the yield.
Smart Images

Figure CN116018884B_ABST
Abstract
Description
Technical Field
[0001] The embodiments described below mainly relate to a bonded body, a ceramic circuit substrate and a semiconductor device using the bonded body. Background Art
[0002] A ceramic copper circuit substrate formed by joining a ceramic substrate and a copper plate is used as a circuit substrate for mounting semiconductor elements, etc. The ceramic copper circuit substrate described in International Publication No. 2017 / 056360 (Patent Document 1) improves the joint body formed by joining a ceramic substrate and a copper plate via a joining layer. In Patent Document 1, a protrusion is provided so that the joining layer protrudes from the end of the copper plate. The TCT characteristics are improved by controlling the size of such a protruding portion of the joining layer.
[0003] In Patent Document 1, an etching process is used to control the size of the protruding portion of the bonding layer. The etching process is a process for removing the copper plate or bonding layer of the bonded body. The bonding layer of Patent Document 1 contains Ag, Cu and Ti. The bonding layer containing Ag, Cu and Ti is formed by an active metal bonding method. When the size of the protruding portion of the bonded body in the etching process is controlled, the yield rate may not be good.
[0004] For example, Japanese Patent No. 3302714 (Patent Document 2) shows a conceptual diagram of a bonding layer structure containing Ag, Cu, and Ti. In the bonding layer structure of Patent Document 2, Ag, Cu, and AgCu eutectic exist.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2017 / 056360
[0008] Patent Document 2: Japanese Patent No. 3302714
[0009] Patent Document 3: International Publication No. 2019 / 054294 Summary of the invention
[0010] Problem that the invention aims to solve
[0011] In the bonding layer formed by the active metal bonding method, Ag and Cu are mixed. In the mixed structure, the removal effect of the etching solution varies. This is because the etching effect is different in the area with more Ag and the area with less Ag. As a result, the size of the protrusion of the bonding layer varies.
[0012] The bonded body according to the embodiment is designed to address such a problem, and is characterized in that the Ag distribution in the bonding layer is controlled.
[0013] Means for solving problems
[0014] The embodiment involves a joint body in which a metal plate and a ceramic substrate are joined via a joining layer containing Ag, and is characterized in that: in a measurement area formed by the length in the thickness direction of the joining layer and its orthogonal direction in a cross section formed by the length in the thickness direction of the joining layer × the length in the orthogonal direction of 200 μm, the Ag-rich region with an Ag concentration of more than 60 at% exists in an area ratio of less than 70% relative to the Ag-poor region with an Ag concentration of less than 50 at%. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a side view showing an example of a joined body according to the embodiment.
[0016] Figure 2 It is a cross-sectional view showing an example of an Ag-rich region and an Ag-poor region in the bonding layer.
[0017] Figure 3 It is a side view showing an example of the ceramic copper circuit board according to the embodiment.
[0018] Figure 4 It is a side view showing an example of a semiconductor device according to an embodiment. DETAILED DESCRIPTION
[0019] A bonded body according to an embodiment is a bonded body formed by bonding a metal plate and a ceramic substrate via a bonding layer containing Ag, and is characterized in that:
[0020] In the measurement area formed by the length in the thickness direction of the bonding layer and its orthogonal direction, which is 200 μm long by the length in the thickness direction of the bonding layer, the Ag-rich region with an Ag concentration of more than 60 at% accounts for less than 70% in terms of area ratio relative to the Ag-poor region with an Ag concentration of less than 50 at%.
[0021] Figure 1 An example of a conjugate is shown in FIG. Figure 1 In the figure, 1 is a bonded body, 2 is a ceramic substrate, 3 is a metal plate, and 4 is a bonding layer. Figure 1 The joint body 1 is formed by placing metal plates 3 on both sides of a ceramic substrate 2 via a joint layer 4. In addition, the metal plates of the ceramic substrate 2 and the copper plate 3 are made to have the same size. The joint body involved in the embodiment is not limited to such a form, and may also be a structure in which a metal plate is provided on one side. Furthermore, Figure 1In the embodiment, the thickness direction of the ceramic substrate 2, the copper plate 3 and the bonding layer 4 is defined as the Z-axis direction, the longitudinal direction is defined as the X-axis direction, and the transverse direction is defined as the Y-axis direction. In addition, the longitudinal and transverse dimensions (the length in the X-axis direction and the length in the Y-axis direction) of the ceramic substrate 2 may be different, and the longitudinal and transverse dimensions of the metal plate 3 may also be different.
[0022] As the ceramic substrate 2, silicon nitride substrates, aluminum nitride substrates, aluminum oxide substrates, aluminum oxide zirconia (アルジル) substrates, etc. can be cited. The length of the thickness direction (i.e., Z-axis direction) of the ceramic substrate 2 (hereinafter referred to as "thickness") is preferably 0.1 mm or more and 1 mm or less. This is because if the thickness of the ceramic substrate 2 is less than 0.1 mm, there is a concern that the strength will decrease. In addition, if the thickness of the ceramic substrate 2 is greater than 1 mm, the ceramic substrate 2 becomes a thermal resistor, and there is a possibility that the heat dissipation of the joint 1 is reduced.
[0023] In addition, when the ceramic substrate 2 is a silicon nitride substrate, the silicon nitride substrate is preferably a substrate having a three-point bending strength of 600 MPa or more. In addition, the thermal conductivity is preferably 80 W / m·K or more. By increasing the strength of the silicon nitride substrate, the thickness of the substrate can be reduced. Therefore, the silicon nitride substrate preferably has a three-point bending strength of 600 MPa or more, and more preferably 700 MPa or more. The silicon nitride substrate can reduce the substrate thickness to less than 0.40 mm, and can further be reduced to less than 0.30 mm.
[0024] When the ceramic substrate 2 is an aluminum nitride substrate, the three-point bending strength of the aluminum nitride substrate is about 300 to 450 MPa. On the other hand, the thermal conductivity of the aluminum nitride substrate is 160 W / m·K or more. Since the aluminum nitride substrate has low strength, the substrate thickness is preferably 0.60 mm or more.
[0025] In addition, when the ceramic substrate 2 is an alumina substrate, the three-point bending strength of the alumina substrate is about 300 to 450 MPa, but it is relatively cheap. In addition, the ceramic substrate 2 can also be an alumina zirconia substrate. The three-point bending strength of the alumina zirconia substrate is as high as about 550 MPa, but the thermal conductivity is in the range of 30 to 50 W / m·K. The so-called alumina zirconia substrate is a substrate formed by a sintered body mixed with alumina and zirconia.
[0026] In addition, as the ceramic substrate 2, any one of a silicon nitride substrate and an aluminum nitride substrate is preferred. The silicon nitride substrate and the aluminum nitride substrate are nitride ceramic substrates. Nitride ceramics react with an active metal brazing material containing Ti to form titanium nitride. In addition, oxide ceramics react with an active metal brazing material containing Ti to form titanium oxide.
[0027] In addition, the metal plate 3 is preferably one selected from a copper plate, a copper alloy plate, an aluminum plate, and an aluminum alloy plate. In addition, the metal plate 3 is preferably a copper plate or a copper alloy plate. Generally speaking, the thermal conductivity of copper is about 400W / m·K, and the thermal conductivity of aluminum is about 240W / m·K. The copper plate can improve the heat dissipation of the circuit substrate due to its high thermal conductivity. In addition, the thickness of the metal plate 3 can also be more than 0.3mm, and can also be further more than 0.6mm. The heat dissipation of the joint body can be improved by thickening the metal plate 3.
[0028] Furthermore, the copper plate is preferably oxygen-free copper. As shown in JIS-H-3100, oxygen-free copper has a copper purity of 99.96 mass % (wt %) or more.
[0029] Here, the cross section is set by the thickness direction of the bonding layer 4 and the orthogonal direction thereof. Moreover, it is characterized in that: in the measurement area formed by the thickness of the bonding layer 4 × the length of 200 μm in the orthogonal direction in the cross section of the bonded body 1, the Ag-rich area with an Ag concentration of 60 at% or more exists at an area ratio of less than 70% relative to the Ag-poor area with an Ag concentration of less than 50 at%. Furthermore, the thickness direction of the bonding layer 4 is equivalent to the Z-axis direction. On the other hand, the orthogonal direction to the thickness direction is equivalent to a direction that can be obtained in a plane (i.e., an XY plane) containing the X-axis and the Y-axis, such as the X-axis direction or the Y-axis direction.
[0030] The bonding layer 4 contains Ag (silver), Cu (copper) and Ti (titanium). Ti is an active metal and easily reacts with the ceramic substrate 2. The bonding method using the solder containing Ti is called the active metal bonding method. The active metal bonding method forms a Ti reaction layer 5 (see FIG. 5 ) on the surface of the ceramic substrate 2. Figure 2 The bonding strength is improved by forming the Ti reaction layer 5. For example, when the ceramic substrate 2 is a nitride-based ceramic substrate, a layer mainly composed of titanium nitride (TiN) is formed on the surface of the ceramic substrate 2. In addition, when the ceramic substrate 2 is an oxide-based ceramic substrate, a layer mainly composed of titanium oxide (TiO 2 The layer mainly composed of titanium nitride or titanium oxide formed on the surface of the ceramic substrate 2 becomes the Ti reaction layer 5.
[0031] The bonding layer 4 is provided between the ceramic substrate 2 and the metal plate 3. The boundary between the ceramic substrate 2 and the bonding layer 4 becomes the boundary between the ceramic substrate 2 and the Ti reaction layer 5 (see Figure 2 ) boundary. As long as nitrogen is detected by EDX area analysis, the layer with titanium as the main component can be regarded as Ti nitride. In addition, when it is difficult to distinguish the boundary between the ceramic substrate 2 and the bonding layer 4, TEM (transmission electron microscope) analysis can be used. According to the results of TEM analysis, the method of detecting Ti and N by performing EDX point analysis on the bonding layer 4 is effective. Regarding oxygen, it can also be measured by the same method.
[0032] In addition, the boundary between the bonding layer 4 and the metal plate 3 is the farthest point in the region where the bonding layer 4 is in contact with the metal plate 3 in the measurement region (the farthest point from the ceramic substrate 2). In addition, the so-called bonding layer 4 is in contact with the metal plate 3 in the region where the bonding layer 4 is in contact with the metal plate 3 in the measurement region. For example, when the metal plate 3 is a copper plate, the farthest point in the region where the Ag component is in contact with the metal plate 3 in the measurement region is 5 at% or more.
[0033] The amount of Ag in the bonding layer 4 can be measured by EDX (energy dispersive X-ray) analysis. EDX analysis is performed on a measurement area formed by the thickness of the bonding layer 4 × the length of 200 μm in the direction orthogonal to the thickness direction, and area analysis is performed within a unit area with the measurement area as a unit area. In addition, EDX is sometimes referred to as EDS.
[0034] In addition, the measurement of EDX may be performed by SEM-EDX, and as SEM, FE-SEM (Field Emission Scanning Electron Microscope: Field Emission SEM) may be used.
[0035] As the FE-SEM, JSM-7200F manufactured by JEOL Ltd. or an apparatus having equivalent performance was used. As the EDX, EX-74600U4L2Q manufactured by JEOL Ltd. or an apparatus having equivalent performance was used.
[0036] First, the area analysis is performed on the thickness of the bonding layer 4 × the length of 200 μm in the direction orthogonal to the thickness direction by EDX. The unit area of the area analysis is defined as the thickness of the bonding layer 4 × the length of 200 μm in the direction orthogonal to the thickness direction because this is a range suitable for investigating the distribution of the bonding layer components. In addition, the area analysis based on SEM-EDX preferably uses a drawing function. Using the color drawing of Ag, areas with high Ag concentration and areas with low Ag concentration are selected for concentration analysis. In this way, the area ratio (%) of the Ag-rich area to the Ag-poor area can be determined. Select 9 μm from the color drawing. 2 The Ag concentration in the area with high Ag concentration above 9 μm can be analyzed. This can be regarded as the Ag concentration in the Ag-rich region. 2 The Ag concentration in the area with low Ag concentration is analyzed and can be regarded as the Ag concentration in the Ag-poor area.
[0037] The junction body 1 is characterized in that, when analyzing the Ag amount in the measurement area of the junction layer 4, in the measurement area of the junction layer 4, the area ratio of the Ag-rich region to the Ag-poor region (hereinafter referred to as "the area ratio of the Ag-rich region") is less than 70%. In the junction body 1 involved in the embodiment, the area ratio of the Ag-rich region is less than 70% regardless of where the junction layer 4 is measured. Therefore, the area ratio (%) of the Ag-rich region to the Ag-poor region can be calculated by the area ratio (%) of the Ag-rich region to the Ag-poor region = [area of the Ag-rich region / (thickness of the junction layer 4 × area of 200 μm in the orthogonal direction of the thickness direction)] × 100 (%).
[0038] Figure 2 An example of a partial cross section of the bonded body 1 is schematically shown in FIG. Figure 2 In the figure, 2 is a ceramic substrate, 3 is a metal plate, 4 is a bonding layer, 5 is a Ti reaction layer, 6 is an Ag-rich region, and 7 is an Ag-poor region. Figure 2 The cross section shown is formed by the thickness direction of the bonding layer 4, i.e., the Z-axis direction, and the orthogonal direction (e.g., the Y-axis direction) relative to this direction. In this cross section, a measurement area of 200 μm in the orthogonal direction (e.g., the Y-axis direction) of the thickness of the bonding layer 4 × the thickness direction, and a three-connected measurement area in which three measurement areas are connected in the orthogonal direction (e.g., the Y-axis direction) are set. When the ceramic substrate 2 is a silicon nitride substrate, the Ti reaction layer 5 becomes a titanium nitride (TiN) layer.
[0039] The titanium nitride of the Ti reaction layer 5 mainly contains titanium nitride in which the atomic ratio of Ti to N is 1:1. The titanium nitride of the Ti reaction layer 5 may contain titanium nitride in which the atomic ratio of Ti to N is other than 1:1.
[0040] If the ceramic substrate 2 is an oxide-based ceramic substrate, the Ti reaction layer 5 becomes titanium oxide (TiO 2 ) layer. In the titanium oxide layer, titanium oxide in which the atomic ratio of Ti to O is 1:2 is the main component. In addition, titanium oxide in the Ti reaction layer 5 may contain titanium oxide in which the atomic ratio of Ti to O is other than 1:2.
[0041] First, there is an Ag-rich region 6 having an Ag concentration of 60 at% or more. In the future, the Ag-rich region having an Ag concentration of 60 at% or more may be described as only an Ag-rich region. The presence of the Ag-rich region 6 can improve the bonding strength. In addition, by making the area ratio of the Ag-rich region in the measurement area less than 70%, the etching property can be improved. As shown in Patent Document 1, the TCT characteristics of the joint body are improved by making the bonding layer protrude from the end of the metal plate 3. The protrusion is controlled to a protrusion amount corresponding to the thickness of the bonding layer 4. The protrusion is formed by etching. Etching is a process of dissolving unnecessary areas using a chemical solution. The chemical solution used in etching is a chemical solution that dissolves Cu and Ag at different rates. Generally speaking, Cu is an element that is easily etched, and Ag is an element that is difficult to etch. Therefore, the Ag-rich region is a region that is difficult to etch. By making the area ratio of the Ag-rich region in the measurement area less than 70%, the area ratio of the region that is difficult to etch can be reduced. As a result, the shape of the protrusion during etching is easy to be neat. Therefore, the area ratio of the Ag-rich region in the measurement area is preferably 70% or less, and more preferably 50% or less. Furthermore, the lower limit of the area ratio of the Ag-rich region in the measurement area is preferably 20% or more. This is because if the Ag-rich region per unit area is less than 20%, there is a possibility that the bonding strength will decrease.
[0042] In addition, it is preferred that the Ag-rich region 6 is located on the Ti reaction layer 5, that is, in contact with the Ti reaction layer 5. The etching process is performed from the metal plate 3 side. This is because if the Ag-rich region 6 exists on the metal plate 3 side, there is a possibility that the etching efficiency of the bonding layer 4 will decrease. When there are multiple Ag-rich regions 6 in the measurement area, it is preferred that 80% or more and 100% or less of the total area of the Ag-rich regions 6 exist on the Ti reaction layer 5.
[0043] In addition, the measurement area is set to be three consecutive three-way measurement areas in the direction orthogonal to the thickness direction. When measuring the Ag distribution in the three-way measurement area, in the thickness direction of the bonding layer 4, there is preferably at least one Ag-poor area with an Ag concentration of less than 50at% in the thickness direction that is continuous in the thickness direction. Here, the so-called measurement area is the range of the thickness of the bonding layer 4 × the length of 200μm in the direction orthogonal to the thickness direction. The so-called measurement of the three-way measurement area means measuring three areas of the thickness of the bonding layer 4 × the length of 200μm in the direction orthogonal to the thickness direction. Hereinafter, the Ag-poor area 7 with an Ag concentration of less than 50at% is sometimes described only as the Ag-poor area 7.
[0044] The Ag concentration of the Ag-poor region 7 is less than 50%, indicating that there are more elements other than Ag. The Ag concentration of the Ag-poor region is preferably less than 50at%, more preferably less than 40at%. The Ag-poor region is an area that is easier to etch than the Ag-rich region. By having at least one Ag-poor region in the triple measurement area, the etching property of the bonding layer 4 can be improved. The presence or absence of the Ag-poor region in the triple measurement area can be measured by color mapping of EDX. In addition, no matter where the triple measurement area of the bonding layer 4 is measured, it is preferred that there is an area where the Ag-poor region is connected in the thickness direction.
[0045] Furthermore, there is sometimes a region where the Ag concentration exceeds 50at% and is less than 60at%. The region where the Ag concentration exceeds 50at% and is less than 60at% is called the Ag intermediate region. The Ag intermediate region is preferably in the range of 0% to 20% by area ratio. If the Ag intermediate region exceeds 20% by area ratio, there is a possibility that the effect of increasing the Ag-poor region is insufficient. Therefore, the Ag intermediate region is preferably 0% to 20% by area ratio, and more preferably 0% to 10% by area ratio. The most preferred Ag intermediate region is 0%.
[0046] In addition, the thickness of the bonding layer 4 is preferably in the range of 10 μm or more and 60 μm or less. The thickness of the bonding layer 4 is the length from the boundary between the ceramic substrate 2 and the bonding layer 4 to the boundary between the bonding layer 4 and the metal plate 3. If the thickness of the bonding layer 4 is 10 μm or more and 60 μm or less, both bonding strength and etching properties can be achieved.
[0047] If the thickness of the bonding layer 4 is less than 10 μm, the bonding layer 4 is too thin, and it is likely that it will be difficult to control the area ratio of the Ag-rich region to less than 70%. In addition, if the thickness of the bonding layer 4 exceeds 60 μm, it is likely to become a major cause of cost increase due to the increase in etching amount. Therefore, the thickness of the bonding layer 4 is preferably greater than 10 μm and less than 60 μm, and more preferably greater than 15 μm and less than 40 μm.
[0048] The boundary between the ceramic substrate 2 and the bonding layer 4 is the boundary between the ceramic substrate 2 and the Ti reaction layer 5. The boundary between the bonding layer 4 and the metal plate 3 is the farthest from the region where the Ag concentration of the bonding layer 4 is 5 at% or more as described above.
[0049] In addition, the bonding layer 4 contains Sn or In, and the concentration of Sn or In in the measurement area is preferably in the range of more than 1at% and less than 6at%. The measurement area here is the area formed in the cross section formed by the thickness direction of the bonding layer 4 and its orthogonal direction, and is the thickness of the bonding layer 4 × the length of 200μm in the orthogonal direction of the thickness direction (square or rectangular). By containing Sn (tin) or In (indium) in the bonding layer 4, the melting point of the solder constituting the bonding layer 4 can be lowered. In addition, by containing Sn and In, Ag-rich regions and Ag-poor regions are easily formed. The bonding layer 4 contains Ag, Cu and Ti. Ag and Cu are elements that easily form eutectics. AgCu eutectic is relatively stable near the atomic ratio of Ag:Cu=7:3. Therefore, it becomes a bonding layer with more Ag-rich regions. If Sn or In is contained, Ag-poor regions are easily formed due to the formation of compounds with Ag and Cu.
[0050] In addition, the concentration of Sn or In in the measurement area is preferably 1 at% or more and 6 at% or less. If the concentration of Sn or In is less than 1 at%, the effect of inclusion may be insufficient. In addition, if the concentration of Sn or In increases to more than 6 at%, the amount of Ag-rich region formed may be insufficient.
[0051] In addition, no matter where the bonding layer 4 is measured, the concentration of Sn or In in the measurement area is preferably within a range of 1 at% or more and 6 at% or less. This indicates that even if Ag-rich and Ag-poor regions are formed, the distribution of Sn or In does not deviate greatly. In other words, Sn or In plays a role in controlling the area ratio of the Ag-rich region.
[0052] Furthermore, C (carbon) may be contained in the joining layer 4. Carbon has an effect of suppressing the wetting and spreading of the joining brazing material.
[0053] The bonded body 1 described above is suitable for a ceramic circuit board. Figure 3 An example of a ceramic circuit substrate is shown in FIG. Figure 3 In the figure, 10 is a ceramic circuit substrate, 8 is a circuit unit, and 9 is a heat sink. Figure 3 In the figure, 1 is a bonded body, 2 is a ceramic substrate, 3 is a metal plate, and 4 is a bonding layer. Figure 3 In the embodiment, by Figure 3 The circuit portion 8 is formed by giving a pattern to the metal plate 3 (upper side in the middle). As a method for forming the circuit portion 8, a method of joining metal plates using solder, a metallization method using metal solder paste, etc. can be cited. Figure 3 In the inner side of the joint body 1 ( Figure 3 A heat sink is bonded to the metal plate 3 (lower side in the figure), but a circuit portion 8 may be bonded to both the front and back sides. In addition, the number and size of the circuit portion 8 may be changed as needed.
[0054] The ceramic circuit substrate 10 needs to be formed into a pattern shape corresponding to the purpose. Etching is effective for forming the pattern shape. The joint body 1 involved in the embodiment is suitable for etching. In addition, the ceramic circuit substrate 10 with a protrusion that makes the joint layer 4 protrude from the end of the metal plate 3 is suitable. In addition, an inclined structure can also be given to the side of the metal plate 3.
[0055] In addition, the bonding strength of the metal plate 3 can be set to 16 kN / mm or more. The bonding strength can be measured by a peel test. As a sample for the peel test, a sample in which a strip-shaped metal plate is bonded to a ceramic substrate can be used. It is preferred that the metal plate 3 is bonded in such a way that one end of the metal plate 3 protrudes from the ceramic substrate 2. The peel strength can be measured by vertically stretching the protruding metal plate 3.
[0056] When no protruding metal plate 3 is formed, the metal plate 3 is pulled so as to be peeled off at the end. When a plurality of metal plates 3 are bonded, the metal plate 3 close to the creeping surface of the ceramic substrate 2 is used for the peeling test.
[0057] Furthermore, the ceramic circuit board 10 according to the embodiment can be used for a semiconductor device having a semiconductor element mounted thereon. Figure 4 An example of a semiconductor device according to an embodiment is shown in FIG. Figure 4 In the figure, 8 is a circuit part, 9 is a heat sink, 10 is a ceramic circuit substrate, 20 is a semiconductor element, and 30 is a semiconductor device. The semiconductor element 20 is bonded to the surface of the circuit part 8 of the ceramic circuit substrate 10 via a bonding layer ( Figure 4 The middle is the upper side). Figure 4 , an example in which one semiconductor element 20 is mounted is shown, but a plurality of semiconductor elements 20 may be mounted. In addition, in the circuit portion 8, in addition to the semiconductor element 20, a lead frame, metal terminals, wire bonding, etc. (not shown) may be joined.
[0058] Next, a method for producing the bonded body 1 according to the embodiment will be described. The method for producing the bonded body 1 according to the embodiment is not limited as long as it has the above-mentioned configuration, but in order to produce it with a high yield, the method for producing it is as follows.
[0059] First, a ceramic substrate 2 is prepared. Examples of the ceramic substrate 2 include a silicon nitride substrate, an aluminum nitride substrate, an aluminum oxide substrate, an alumina zirconia substrate, etc. The thickness of the ceramic substrate 2 is preferably 0.1 mm or more and 1 mm or less.
[0060] In addition, when the ceramic substrate 2 is a silicon nitride substrate, the three-point bending strength of the ceramic substrate 2 is preferably greater than 600 MPa. In addition, the thermal conductivity is preferably greater than 80 W / m·K. By increasing the strength of the silicon nitride substrate, the substrate thickness can be reduced. Therefore, the three-point bending strength of the silicon nitride substrate is preferably greater than 600 MPa, and more preferably greater than 700 MPa. The silicon nitride substrate can reduce the substrate thickness to less than 0.40 mm, and further to less than 0.30 mm. In addition, the vertical and horizontal dimensions of the ceramic substrate 2 can also be a large substrate that can be processed in multiple pieces at the same time. In addition, the vertical and horizontal dimensions of the ceramic substrate 2 can also be the dimensions used as a ceramic circuit substrate 10.
[0061] Next, prepare the metal plate 3. The metal plate 3 is preferably one selected from a copper plate, a copper alloy plate, an aluminum plate, and an aluminum alloy plate. In addition, the thickness of the metal plate 3 is preferably 0.3 mm or more, and more preferably 0.6 mm or more. Furthermore, there is no particular upper limit on the thickness of the metal plate 3, but it is preferably 2 mm or less. If the thickness of the metal plate 3 exceeds 2 mm, it is possible that the etching process is difficult. In addition, the vertical and horizontal dimensions of the metal plate 3 may also be the same as those of the ceramic substrate 2. In addition, a metal plate pre-processed into a pattern shape may also be used.
[0062] Next, a process of preparing a solder for bonding is performed. The solder for bonding has Ag (silver), Cu (copper) and Ti (titanium) as essential components. In addition, one or more selected from Sn (tin), In (indium) and C (carbon) may be added as needed.
[0063] Ag and Cu are components that form the matrix of the bonding layer 4. Ti is a component that forms the Ti reaction layer 5 by reacting with the ceramic substrate 2. Ti can also be a Ti single substance or titanium hydride (TiH 2 ). In addition, Sn or In has the effect of lowering the melting point of the solder. In addition, C (carbon) can control the fluidity of the solder.
[0064] In addition, Ag is preferably in the range of 20 mass % or more and 60 mass % or less, and Cu is preferably in the range of 15 mass % or more and 40 mass % or less. Ti or TiH 2 One or two of Sn (tin) and In (indium) are preferably in a range of 1 mass % to 15 mass %. In addition, one or two of Sn (tin) and In (indium) are preferably in a range of 1 mass % to 50 mass %. C (carbon) is preferably in a range of 0.01 mass % to 2 mass %.
[0065] The ratio of the brazing material composition can be calculated by taking the total of the mixed raw materials as 100 mass %. For example, when the brazing material is composed of Ag, Cu, and Ti, it is Ag+Cu+Ti=100 mass %. In addition, when the brazing material is composed of Ag, Cu, TiH2 , In four kinds of composition, Ag+Cu+TiH 2 +In=100 mass %. When composed of five elements, Ag, Cu, Ti, Sn, and C, it is Ag+Cu+Ti+Sn+C=100 mass %.
[0066] Furthermore, the particle size of the raw material powder of the brazing material is preferably as follows.
[0067] The average particle size of Ag powder 50 Preferably, the Cu powder has an average particle size D of 3.0 μm or less. 50 It is preferably 12.0 μm or less, and more preferably 10.0 μm or less. 2 The average particle size of the powder is D 50 Preferably, the average particle size D of the Sn powder or In powder is 6.0 μm or less. 50 The average particle size D of the carbon powder is preferably 16.0 μm or less, and more preferably 14.0 μm or less. 50 It is preferably 3.0 μm or less.
[0068] In addition, the Ag particle size D 50 The thickness is preferably 1.5 μm or more and 3.0 μm or less, and more preferably 1.8 μm or more and 2.8 μm or less.
[0069] In addition, the particle size D of the Ag powder 10 Preferably, the particle size D of the Ag powder is 1.0 μm or more. 90 It is preferably 3.5 μm or less. 50 After the particle size D is 3.0 μm or less, it is preferred that the particle size D 10 1.0 μm or more, particle size D 90 By controlling D 10 , D 50 , D 90 , and become Ag powder with uniform particle size. Ag powder with uniform particle size becomes powder with steep particle size distribution. As a result, Ag powder is easy to agglomerate and form Ag-rich area.
[0070] In addition, the tap density of the Ag powder is preferably 4.5 g / cm 3 The tap density is the value obtained by dividing the mass of the powder sample by the tap volume. The tap volume is obtained by measuring the inter-particle gaps generated by lifting a container containing a powder sample to a certain distance and letting it fall. The tap density can be measured in accordance with JIS-Z-2512 (2012). The ISO corresponding to JIS-Z-2512 is ISO 3953 (2011).
[0071] The tap density indicates the fluidity of the powder. If the tap density is large, the fluidity of the powder is good. By improving the fluidity, the Ag powder can be coated in its original state while maintaining its coagulated state. Thus, the Ag-rich region 6 is easily formed. Therefore, the tap density of the Ag powder is preferably 4.5 g / cm 3 More preferably, 4.8 g / cm 3 The upper limit of the tap density of the Ag powder is not particularly limited, but is preferably 6.2 g / cm 3 If it exceeds 6.2g / cm 3 This may become a major cause of cost increase.
[0072] In addition, the content of Na (sodium), K (potassium), and Cl (chlorine) in the Ag powder is preferably 0.005 mass % or less in total. In addition, it is preferably 0.002 mass % or less respectively. Na, K, and Cl are impurities. If these elements are more, there is a possibility that the reactivity in the heating bonding process is reduced.
[0073] With the above-described configuration, the Ag-rich region 6 can be easily formed in the bonding layer 4 .
[0074] The constituent powders of the brazing material are mixed and uniformly dispersed to prepare a mixed powder. In addition, the mixing step of the constituent powders is preferably performed for 10 hours or more.
[0075] Next, the mixed powder is mixed with a binder or a solvent to prepare a solder paste. In addition, it is preferred that the mixing step of the mixed powder and the binder etc. is also performed for 10 hours or more.
[0076] The solder paste is applied on at least one of the ceramic substrate or the copper plate. The thickness of the solder paste layer is preferably greater than 5 μm and less than 60 μm. The thickness of the solder paste layer is the thickness after the applied solder paste is dried. If the thickness is less than 5 μm, there is a possibility that the bonding strength decreases. In addition, if the thickness exceeds 60 μm, the bonding layer 4 is thickened, and there is a possibility of increasing the etching load. Therefore, the thickness of the solder paste layer is preferably greater than 5 μm and less than 60 μm, and more preferably greater than 10 μm and less than 50 μm.
[0077] After the solder paste coating process is performed, a process of arranging the side not coated with solder paste is performed. For example, if the solder paste is coated on a ceramic substrate, it is a process of arranging a copper plate. In addition, the solder paste may be coated on both sides of the ceramic substrate and the copper plates may be arranged on both sides. In addition, the solder paste may be coated on the copper plate and the ceramic substrate may be arranged.
[0078] Next, a heat bonding step is performed. The heating temperature is preferably 720°C or higher and 920°C or lower. -3Pa or less in vacuum.
[0079] Through the above process, the joint body 1 can be manufactured. In addition, the ceramic circuit substrate 10 can be manufactured by etching the joint body 1. Any method can be used for the etching process. In addition, as an example of the etching process, International Publication No. 2019 / 054294 (Patent Document 3) can be cited. In the etching process of the joint body 1 manufactured by the active metal bonding method, it is necessary to perform the etching process of the metal plate 3, the etching process of the bonding layer 4, and the etching process of the Ti reaction layer 5. The joint body 1 involved in the embodiment controls the distribution of the Ag-rich region 6, so that the processing speed of the etching process of the bonding layer 4 can be increased. In addition, the etching rate of the etching process of the bonding layer 4 can be stabilized. Thus, the deviation of the size of the protrusion of the bonding layer 4 can be reduced. As mentioned above, the ceramic circuit substrate 10 involved in the embodiment can improve the bonding strength of the metal plate 3. That is, the etching property can be improved while maintaining the bonding strength.
[0080] Furthermore, after the etching process, scribing is performed as necessary to perform simultaneous processing of multiple pieces.
[0081] (Example)
[0082] (Examples 1 to 10, Comparative Example 1)
[0083] As ceramic substrates, silicon nitride substrates, aluminum nitride substrates, and alumina zirconia substrates were prepared. The silicon nitride substrate was set to 200 mm in length × 160 mm in width × 0.32 mm in thickness, and a thermal conductivity of 90 W / m·K. The aluminum nitride substrate was set to 200 mm in length × 160 mm in width × 0.635 mm in thickness, and a thermal conductivity of 170 W / m·K. The alumina zirconia substrate was set to 200 mm in length × 160 mm in width × 0.635 mm in thickness, and a thermal conductivity of 20 W / m·K.
[0084] In addition, copper plates were prepared as metal plates. The first copper plate was set to 200 mm in length×160 mm in width×0.8 mm in thickness. The second copper plate was set to 200 mm in length×160 mm in width×0.3 mm in thickness.
[0085] Next, a brazing material was prepared. The composition of the brazing material is shown in Table 1. In addition, the particle sizes of the constituent components of the brazing material are shown in Tables 2 and 3.
[0086] Table 1
[0087] Brazing material composition [mass %] Brazing material 1 Ag(60)-Cu(25)-Sn(10)-Ti(5) Brazing material 2 <![CDATA[Ag(49.8)-Cu(29)-Sn(13)-TiH 2 (8)-C(0.2)]]> Brazing material 3 <![CDATA[Ag(47.7)-Cu(30)-Sn(15)-TiH 2 (7)-C(0.3)]]> Brazing material 4 Ag(64)-Cu(25)-Sn(8)-Ti(3) Brazing material 5 <![CDATA[Ag(46.9)-Cu(33)-Sn(11)-TiH 2 (9)-C(0.1)]]>
[0088] Table 2
[0089]
[0090] Table 3
[0091]
[0092] As shown in Table 3, solders 1 to 3 and 5 have Ag powder D 10 , D 50 , D 90 And the tap density is controlled within the preferred range. In addition, as shown in Table 3, the brazing material 4 has a tap density lower than 4.5 g / cm 3 The tap density was measured in accordance with JIS-Z-2512 (2012).
[0093] Next, the mixing process of the constituent powders of the mixed solder is carried out for more than 10 hours. Then, the mixed powder is mixed with a binder and a solvent to prepare a solder paste. In addition, the mixing process of the mixed powder and the binder is also carried out for more than 10 hours.
[0094] Next, solder paste is applied to both surfaces of the ceramic substrate, and then the metal plate is placed. The heating bonding step is performed at a temperature in the range of 780°C to 850°C for 10 -3 The process was performed in a vacuum at a pressure of Pa or less. The combinations of the ceramic substrate, the metal plate, and the brazing material are shown in Table 4. Through this process, the bonded bodies according to the examples and comparative examples were manufactured.
[0095] Table 4
[0096] Ceramic Substrate Metal Sheet Brazing material Example 1 Silicon Nitride Substrate Copper Plate 1 Brazing material 1 Example 2 Silicon Nitride Substrate Copper Plate 1 Brazing material 1 Example 3 Silicon Nitride Substrate Copper Plate 1 Brazing material 2 Example 4 Silicon Nitride Substrate Copper Plate 1 Brazing material 2 Example 5 Silicon Nitride Substrate Copper Plate 1 Brazing material 3 Example 6 Silicon Nitride Substrate Copper Plate 2 Brazing material 3 Example 7 Aluminum Nitride Substrate Copper Plate 2 Brazing material 1 Example 8 Silicon Nitride Substrate Copper Plate 1 Brazing material 5 Example 9 Silicon Nitride Substrate Copper Plate 1 Brazing material 5 Example 10 Alumina Zirconia Substrate Copper Plate 2 Brazing material 1 Comparative Example 1 Silicon Nitride Substrate Copper Plate 1 Brazing material 4
[0097] The thickness of the bonding layer and the bonding strength of the metal plate were measured for the bonded bodies obtained according to Examples 1 to 10 and Comparative Example 1 in Table 4. The thickness of the bonding layer was observed in a cross section formed by the thickness direction and the orthogonal direction thereof. In addition, the bonding strength of the metal plate was measured by a peel test. The results are shown in Table 5.
[0098] In addition, the thickness of the bonding layer was measured using the aforementioned method. In addition, in the peel test, the bonding conditions of each embodiment and comparative example were used to prepare a peel test sample. The sample was bonded to a strip copper plate on a ceramic substrate. At this time, the bonding was performed in a manner that one end of the copper plate protruded from the ceramic substrate. The peel strength was measured by vertically stretching the protruding copper plate.
[0099] Table 5
[0100]
[0101] As shown in Table 5, in Examples 1 to 10 and Comparative Example 1, the thickness of the bonding layer is within the range of 10 μm or more and 60 μm or less. In addition, in Examples 1 to 9, a titanium nitride layer is formed as a Ti reaction layer. In Example 10, a titanium oxide layer is formed as a Ti reaction layer.
[0102] Next, in Examples 1 to 10 and Comparative Example 1, the Ag-rich and Ag-poor regions in the measurement area of the thickness of the bonding layer × the length of 200 μm in the orthogonal direction to the thickness direction were measured by EDX analysis, and the area ratio of the Ag-rich region was calculated. In Comparative Example 1, in the measurement area (thickness 18 μm × length 200 μm in the orthogonal direction), the area ratio of the Ag-rich region was the largest (85%). In addition, in Comparative Example 1, in the measurement area, the Ag concentration in the Ag-poor region was the largest (48 at%). In addition, in Examples 1 to 10 and Comparative Example 1, it was confirmed whether there were more than one region in which the Ag-poor region was connected in the thickness direction in the three-connected measurement area. The results are shown in Table 6.
[0103] Table 6
[0104]
[0105] As shown in Table 6, in the joints involved in Examples 1 to 10, the area ratio of the Ag-rich region in the measurement region is less than 70%. In addition, in the joints involved in Examples 1 to 10, even the minimum value of the area ratio of the Ag-rich region in the measurement region is more than 20%. In addition, in the joints involved in Examples 1 to 10, more than 80% of the Ag-rich region is formed on the titanium nitride layer.
[0106] In the junctions according to Examples 1 to 10, the Ag concentration of the Ag-poor region was 50 at% or less even at its maximum value. In the junctions according to Examples 1 to 10, there were regions in which the Ag-poor regions were connected in the thickness direction in the triple measurement regions.
[0107] In contrast, the area ratio of the Ag-rich region in the measurement region was 85% in Comparative Example 1. In Comparative Example 1, no region in which the Ag-poor regions were connected in the thickness direction was found in the three consecutive measurement regions.
[0108] Next, the etching properties of each bonded body were investigated. Regarding the etching process, first, an etching process was performed to give a pattern shape to the copper plate. Multiple locations with a pattern interval of 2 mm were set. Through this process, a bonded body with a bare bonding layer was formed.
[0109] Next, the bonding layer and the titanium nitride layer are etched. In order to etch the bonding layer and the titanium nitride layer, a solution containing hydrogen peroxide (H 2 O 2 ) and ammonium fluoride (NH4 When the etching time required for etching the bonded body of Comparative Example 1 until the ceramic substrate surface is visible is set as 100, the ratio of the etching time required for etching the bonded body of the Example until the ceramic substrate surface is visible is investigated. The results are shown in Table 7.
[0110] Table 7
[0111] Etching time ratio Example 1 83 Example 2 86 Example 3 75 Example 4 77 Example 5 74 Example 6 73 Example 7 75 Example 8 78 Example 9 77 Example 10 86 Comparative Example 1 100
[0112] From Table 7, it can be seen that the joints according to Examples 1 to 10 can shorten the etching time by about 20 to 30% under the same etching conditions compared with Comparative Example 1. In other words, it can be seen that Comparative Example 1 having more Ag-rich regions has a slower etching rate.
[0113] In addition, etching treatment was performed to form a protrusion so that the bonding layer protruded from the end of the metal plate. The desired protrusion amount was set. The protrusion amount after etching was measured at any 10 locations. The minimum and maximum values of the protrusion amount are shown. The results are shown in Table 8.
[0114] Table 8
[0115]
[0116] It can be seen from Table 8 that in the joint bodies involved in Examples 1 to 10, the deviation of the minimum and maximum values (maximum value-minimum value or minimum value-maximum value) relative to the intended protrusion amount is within ±28μm. In contrast, in Comparative Example 1, there is a deviation of more than 30μm. It is known that the joint bodies involved in Examples 1 to 10 can maintain the shape when etching is performed. Therefore, it is known that the joint body 1 involved in the embodiment is suitable for etching.
[0117] Several embodiments of the present invention have been described above, but these embodiments are shown as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other ways, and various omissions, substitutions, and changes can be made without departing from the scope of the main purpose of the invention. These embodiments and their variations are included in the scope and main purpose of the invention, and are also included in the invention described in the claims and their equivalents. In addition, the above-mentioned embodiments can be implemented in a combination with each other.
Claims
1. A bonded body, wherein a metal plate and a ceramic substrate are bonded via a bonding layer containing Ag, characterized in that: In a measurement area formed by the length in the thickness direction of the bonding layer × the length in the orthogonal direction of 200 μm in the cross section formed by the thickness direction and the orthogonal direction of the bonding layer, an Ag-rich region having an Ag concentration of 60 at% or more exists in an area ratio of 70% or less relative to an Ag-poor region having an Ag concentration of 50 at% or less, The bonding layer contains Sn or In, and the concentration of Sn or In in the measurement region is in a range of 1 at % to 6 at %, Among the three consecutive measurement regions in which the measurement regions are three consecutive measurement regions in the orthogonal direction, there is at least one region in which the Ag-poor region is continuous in the thickness direction of the bonding layer.
2. The joint body according to claim 1, characterized in that: The length of the bonding layer in the thickness direction is within a range of 10 μm to 60 μm.
3. The joint body according to claim 1, characterized in that: The ceramic substrate is a silicon nitride substrate, and the metal plate is a copper plate.
4. The joint body according to claim 3, characterized in that: The ceramic substrate is a silicon nitride substrate having a thickness of 0.4 mm or less, and the metal plate is a copper plate having a thickness of 0.5 mm or more.
5. A ceramic circuit substrate, characterized in that: The bonded body according to claim 4 is used.
6. A semiconductor device, characterized in that: The ceramic circuit board according to claim 5 has a semiconductor element mounted thereon.
Citation Information
Patent Citations
Circuit substrate and semiconductor device
WO2017056360A1
Method for manufacturing ceramic circuit board
WO2019054294A1
Bonding body, circuit board and semiconductor device
CN109476556A