A method for online quenching shape control of steel plates with different widths
By adjusting the header water ratio and roller speed in the MULPIC rapid cooling device, combined with the side spraying function, the problem of ultra-wide steel plate shape control is solved, and an efficient online quenching effect is achieved. It is suitable for steel plates with a width of 1800~4000mm. Simplify the process and reduce costs.
Patent Information
- Application Number
- CN202310221033.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-09
AI Technical Summary
The existing online quenching technology is difficult to effectively control the plate shape of ultra-wide steel plates, especially steel plates with a width of more than 3000mm. It is prone to bend deformation during the cooling process, resulting in unqualified plate shapes, and the prior art has failed to target steel plates of different widths. The quenching process and plate shape matching method are disclosed in detail.
The MULPIC rapid cooling device is used to manually adjust the water ratio, water volume and roller speed of the head pipe, and use side spraying and other functions to ensure uniform cooling of the steel plate. The overall cooling temperature is achieved through head and tail shielding, side spraying and purge functions. The uniformity of the lower header/upper header water ratio is adjusted to optimize according to the width of the steel plate to ensure cooling efficiency and quenching effect.
It realizes effective plate shape control of steel plates with widths of 1800~4000mm, ensures that the unevenness of steel plates after quenching is ≤5/1000mm, simplifies the process flow, reduces production costs, is suitable for high-level tempered steel production, has significant market competitiveness and application prospect.
Smart Images

Figure CN116024414B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of steel plate shape control technology, in particular to a method for online quenching shape control of steel plates of different widths. The present invention is particularly directed to a shape control method for online quenching high-strength steel plates with a thickness of 20 to 50 mm and a width of 1800 to 4000 mm. Background Art
[0002] The direct quenching process after rolling is often used in the production of steel grades for engineering machinery with a tensile strength of more than 700-1000MPa. Compared with the traditional offline tempering process, the online quenching process uses a faster cooling rate and a lower terminal cooling temperature after rolling, so that the steel plate does not undergo ferrite and pearlite phase transformation, and directly enters the bainite or martensite transformation zone, forming a microstructure dominated by refined bainite or martensite, which has high strength and toughness. This set of processes omits the reheating austenitization process, saves energy and simplifies the production process, which directly promotes reducing energy consumption, reducing carbon dioxide emissions, and releasing heat treatment capacity. It is a typical green steel manufacturing technology.
[0003] In the actual production process, the online quenched steel plate is easily deformed due to the interaction of thermal stress and phase change stress during the cooling process, which requires the steel plate to be rescued or even scrapped. The shape problem is particularly prominent for steel plates with a width of more than 3000mm. How to ensure the control of quenching shape is the key to realizing online quenching technology.
[0004] The MULPIC rapid cooling device of Ezhou Steel's 4300mm wide and thick plate plant adopts a variable flow water pillow cooling header with edge shielding and water convexity control. There are 24 headers arranged at the top and bottom, divided into 4 zones A, B, C, and D. Each zone is 6m long and has a total length of 24m. It has an online quenching function but does not have an automatic cooling model. It is necessary to manually set process parameters such as cooling area, water volume of each header, upper and lower water ratio, and roller speed according to the performance requirements of each steel grade.
[0005] Existing online quenching plate shape control technologies for high-strength steel, such as the 2009 Chinese patent application (publication number CN101633976A) "A direct quenching process suitable for high-strength and tough steel plates of different thicknesses", mainly introduces the use of high-density laminar cooling to achieve online direct quenching process methods for different thickness specifications, but does not involve the matching method of quenching processes for steel plates of different widths and steel plate shapes; the 2020 Chinese patent application (publication number CN 109266815 B) "Online quenching high-strength steel plate shape control method" introduces the quenching process of 20-80mmQ550 and Q690 steel plates of different thickness specifications at different ambient temperatures, and also does not disclose the method of matching the quenching process and steel plate shape for steel plates of different widths. Summary of the invention
[0006] The purpose of the present invention is to provide a method suitable for online quenching plate shape control of steel plates of different widths. The method of the present invention is suitable for online quenching plate shape control of high-strength engineering machinery steel with a thickness of 20 to 50 mm, a width of 1800 to 4000 mm, and a tensile strength of 1000 MPa. The method of the present invention adopts a MULPIC rapid cooling device to manually adjust the upper and lower water ratio, water volume and roller speed of the header, and utilizes functions such as side spraying to ensure uniform cooling of the steel plate and achieve quenching effect, and the plate shape is qualified.
[0007] A method for online quenching shape control of steel plates with different widths according to the present invention comprises the following steps:
[0008] (1) Converter smelting and continuous casting into billets;
[0009] (2) The temperature of continuous casting billet out of furnace is 1180~1240℃;
[0010] (3) Rolling process: A two-stage rolling process is adopted to control the final rolling temperature of the steel plate to 850-910°C;
[0011] (4) Cooling process: After the pre-straightening machine, the steel plate enters the MULPIC device for quenching cooling. The start cooling temperature is 800-850°C, the roller speed is 0.5-1.2 m / s, the header is used for regional spraying, the lower header / upper header water ratio is 1.1-1.5, and the cooling rate is 20-38°C / s; the steel plate cooling end temperature is 50-120°C; the upper and lower header water ratio is determined according to the width of the steel plate, and the specific control method is as follows:
[0012] A. For steel plate widths between 1800 and 2500 mm, set the lower header / upper header water ratio between 1.32 and 1.5;
[0013] B. For steel plate widths between 2500 and 3200 mm, set the lower header / upper header water ratio between 1.21 and 1.45;
[0014] C. For steel plate widths between 3200 and 4000 mm, set the lower header / upper header water ratio between 1.1 and 1.40;
[0015] (5) After quenching of the steel plate, it is sent to the heat treatment furnace for tempering heat treatment.
[0016] The cooling process of the present invention adopts the DQ cooling mode of the MULPIC device for quenching cooling.
[0017] The cooling process of the present invention adopts head and tail shielding, side spraying and purging functions to ensure the uniformity of the overall cooling temperature of the steel plate.
[0018] In order to ensure the cooling efficiency of the steel plate, the present invention adopts a cooling fan device to ensure that the water temperature is ≤26°C.
[0019] The finished steel plate prepared by the invention has a thickness of 20 to 50 mm, a width of 1800 to 4000 mm, and a tensile strength of 900 to 1000 MPa.
[0020] The reasons for controlling the main process parameters in the method of the present invention are as follows:
[0021] (1) After the steel plate is rolled, it needs to go through a pre-straightening process to ensure that the steel plate is straight before entering rapid cooling, providing a good plate shape for subsequent uniform deformation of the steel plate;
[0022] (2) In order to prevent water accumulation on the steel plate and uneven cooling and deformation, the head and tail shielding, side spraying and blowing functions of the MULPIC device must be used;
[0023] (3) Due to the effect of gravity, the cooling water retention time on the upper and lower surfaces of the steel plate is different. Under the same water volume and water ratio, the cooling degree of the upper surface is higher than that of the lower surface. The cooling efficiency of the water on the lower surface of the steel plate is lower than that on the upper surface. Therefore, the overall water volume process is that the lower water volume is higher than the upper water volume, and the lower header / upper header water ratio is 1.1-1.5;
[0024] (4) For steel plates with a width of ≤2500mm, ≤3200mm, and ≤4000mm, the lower header / upper header water ratio gradually decreases. This is because as the width of the steel plate increases, the cooling area increases, the overall cooling efficiency of the steel plate increases, and the cooling intensity of the lower surface of the steel plate increases;
[0025] (5) In order to ensure the cooling effect of the steel plate and the hardenability of the steel plate, the cooling water temperature is required to be controlled at ≤26°C and the actual temperature is controlled at 10~26°C.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The solution of the present invention not only meets the quenching performance requirements of steel plates, but also solves the problem of online quenching plate shape of steel plates of different widths, especially the plate shape unevenness of ultra-wide plates of 3000 to 4000 mm or more after online quenching is ≤5 / 1000mm;
[0028] (2) The plate shape control method of the online quenching high-strength steel plate with a thickness of 20 to 50 mm and a width of 1800 to 4000 mm of the present invention effectively shortens the process flow and production costs. The process is simple and feasible, easy to carry out large-scale production, and can be promoted and applied to the production process of high-level quenched and tempered steel for containers, bridges, platforms, high-rise buildings, etc. It has strong market competitiveness and application prospects, and has obvious economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a photograph of the unevenness measurement of a 30 mm (thickness) × 3800 mm (width) steel plate prepared in Example 7 of the present invention after online quenching. DETAILED DESCRIPTION
[0030] In order to better explain the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with specific embodiments. The following embodiments are merely exemplary of the technical solution of the present invention and do not limit the present invention in any form. Any changes or equivalent substitutions that do not deviate from the concept of the present invention are included in the protection scope of the present invention.
[0031] Table 1 below is a list of main parameter values of the steel rolling and cooling processes of various embodiments of the present invention;
[0032] Table 2 below is a list of specific plate shape control process parameter values for various embodiments of the present invention;
[0033] Table 3 below is a table of the roughness measurements of the finished steel plates produced according to various embodiments of the present invention.
[0034] A method for online quenching shape control of steel plates of different widths according to various embodiments of the present invention comprises the following steps:
[0035] (1) Converter smelting and continuous casting into billets;
[0036] (2) The temperature of continuous casting billet out of furnace is 1180~1240℃;
[0037] (3) Rolling process: A two-stage rolling process is adopted to control the final rolling temperature of the steel plate to 850-910°C;
[0038] (4) Cooling process: After the pre-straightening machine, the steel plate enters the MULPIC device for quenching cooling. The start cooling temperature is 800-850°C, the roller speed is 0.5-1.2 m / s, the header is used for regional spraying, the lower header / upper header water ratio is 1.1-1.5, and the cooling rate is 20-38°C / s; the steel plate cooling end temperature is 50-120°C; the upper and lower header water ratio is determined according to the width of the steel plate, and the specific control method is as follows:
[0039] A. For steel plate widths between 1800 and 2500 mm, set the lower header / upper header water ratio between 1.32 and 1.5;
[0040] B. For steel plate widths between 2500 and 3200 mm, set the lower header / upper header water ratio between 1.21 and 1.45;
[0041] C. For steel plate widths between 3200 and 4000 mm, set the lower header / upper header water ratio between 1.1 and 1.40;
[0042] (5) After quenching of the steel plate, it is sent to the heat treatment furnace for tempering heat treatment.
[0043] Table 1 List of main parameter values of steel rolling and cooling process in various embodiments of the present invention
[0044]
[0045] Table 2 List of specific plate shape control process parameters of various embodiments of the present invention
[0046]
[0047] Table 3 Unevenness measurement list of finished steel plates obtained in various embodiments of the present invention
[0048]
[0049] It can be seen from Tables 1-3 above that after the online quenching process of the present invention, the steel plate has a good shape, the maximum unevenness of the steel plate is 5 mm / m, and after the tempering heat treatment at 550-610°C, the unevenness of the steel plate is ≤3 mm / m. This shows that the method of the present invention has good control over the shape of steel plates of different widths. Figure 1 This is a photo of the unevenness measurement of a steel plate with a thickness of 30 mm and a width of 3800 mm prepared in Example 7 of the present invention. It can be seen from the photo that the unevenness of the steel plate is only 2 mm / m.
[0050] The above embodiments are only the best examples and are not intended to limit the implementation of the present invention.
Claims
1. A method for online quenching shape control of steel plates of different widths, characterized in that The steps include: (1) Converter smelting and continuous casting into billets; (2) The temperature of continuous casting billet out of furnace is 1180~1240℃; (3) Rolling process: A two-stage rolling process is adopted to control the final rolling temperature of the steel plate to 850-910°C; (4) Cooling process: After the pre-straightening machine, the steel plate enters the MULPIC device for quenching cooling. The start cooling temperature is 800-850°C, the roller speed is 0.5-1.2 m / s, the header is used for regional spraying, the lower header / upper header water ratio is 1.1-1.5, and the cooling rate is 20-38°C / s; the steel plate cooling end temperature is 50-120°C; the lower header / upper header water ratio is determined according to the width of the steel plate, and the specific control method is as follows: A. For steel plates with a width of 1800 ≤ steel plate width ≤ 2500 mm, set the lower header / upper header water ratio to 1.32-1.5; B. For steel plates with a width of 2500< steel plate width ≤ 3200mm, set the lower header / upper header water ratio to 1.21~1.45; C. For steel plates with a width of 3200< steel plate width ≤ 4000mm, set the lower header / upper header water ratio to 1.1-1.40; (5) After quenching of the steel plate, it is sent to the heat treatment furnace for tempering heat treatment; To ensure the cooling efficiency of the steel plate, a cooling fan is used to ensure that the water temperature is ≤26°C; The thickness of the finished steel plate is 20-50mm, the width is 1800-4000mm, and the tensile strength of the steel plate is 900-1000MPa; after the online quenching process, the steel plate has a good shape, the maximum unevenness of the steel plate is 5mm / m, and after tempering heat treatment at 550-610℃, the unevenness of the steel plate is ≤3mm / m.
2. The method for online quenching shape control of steel plates of different widths according to claim 1 is characterized in that: The cooling process adopts the DQ cooling mode of the MULPIC device for quenching cooling.
3. The method for online quenching shape control of steel plates of different widths according to claim 1, characterized in that: The cooling process adopts head and tail shielding, side spraying and purging functions to ensure the uniformity of the overall cooling temperature of the steel plate.