A high entropy alloy material and preparation method thereof
Through high-energy ball milling and laser cladding technology of Ti, Mo, Nb, and Cr high-entropy alloy materials, the problem of insufficient performance of titanium alloys in applications is solved, and a coating with high hardness, high-temperature oxidation resistance, and good wear resistance is prepared. , meeting the high-performance needs of aerospace, medical and other fields, and simplifying the preparation process.
Patent Information
- Application Number
- CN202310033761.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-10
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-10
AI Technical Summary
In practical applications, titanium alloys are limited by high friction factors, low high-temperature oxidation resistance, poor wear resistance, and difficulty in lubrication. The preparation process of refractory high-entropy alloys is complex and difficult to control, and cannot meet the high-performance needs of aerospace, medical, etc.
Using high-entropy alloy materials composed of four metal elements: Ti, Mo, Nb, and Cr, the coating is prepared through high-energy ball milling and laser cladding technology to form a cladding layer with high hardness, high-temperature oxidation resistance, and good wear resistance. The base material achieves metallurgical bonding.
It achieves high hardness, high friction and wear resistance and high temperature oxidation resistance, improves the bonding strength between the coating and the substrate, reduces thermal deformation and dilution rate, simplifies the preparation process and improves preparation efficiency.
Smart Images

Figure CN116024480B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high entropy alloy coatings, and in particular relates to a high entropy alloy material and a preparation method thereof. Background Art
[0002] Laser cladding coating is a new application of laser in the field of surface technology. Compared with other coating preparation technologies, laser cladding technology has some unique advantages, such as the metallurgical bonding quality of coating and substrate; the thickness of coating is easy to control; good coating structure is dense, the chemical uniformity of the structure formed after laser melting is very high, and the grains are very fine, thus strengthening the alloy, and the strength and hardness are increased. Therefore, in the field of surface treatment, the research and development of laser cladding has been a hot direction in recent years.
[0003] For traditional alloys, one element is the main element, and a small amount of other elements is added to improve the performance of the alloy. However, due to the influence of solid solubility, the number of added elements is always small, and the performance of the alloy can no longer meet the needs of aerospace, medical equipment, etc. The discovery of high-entropy alloys is a new exploration of the preparation of high-performance alloys. The number of principal elements in high-entropy alloys n ≥ 5, and the content of each element is between 5% and 35at%, but Dr. Senkov of the US Air Force Laboratory believes that NbMoTaW and NbTiVZr quaternary equiatomic ratio alloys are also typical high-entropy alloys.
[0004] Compared with traditional alloys, high entropy alloys have the following characteristics: (1) higher strength and hardness; (2) good corrosion resistance and fatigue resistance; (3) better thermal stability; (4) strong resistance to high temperature oxidation.
[0005] Titanium alloys have the advantages of high specific strength, low density, good corrosion resistance and good biocompatibility, and are widely used in aerospace, biomedicine, petrochemical and other fields. With the development of science and technological progress, the comprehensive performance requirements of titanium alloys are getting higher and higher. However, the disadvantages of titanium alloys such as high friction coefficient, low high-temperature oxidation resistance, severe adhesive wear, poor wear resistance and difficulty in lubrication have greatly limited the scope of use of titanium alloys in practical applications.
[0006] Refractory high entropy alloys are high entropy alloys with high melting point refractory elements added, such as Ti, Cr, Nb, Zr, etc. Their excellent high temperature resistance has attracted research researchers to study them as heat-resistant coatings. However, there are relatively few reports on refractory high entropy alloys. This is mainly because the addition of high melting point elements makes the coating preparation process more difficult to control. However, the excellent high temperature oxidation resistance of refractory high entropy alloys is of great significance in practical applications.
[0007] Therefore, in order to solve the above problems, this paper proposes a high entropy alloy material and a preparation method thereof. Summary of the invention
[0008] In order to solve the above technical problems, the present invention designs a high entropy alloy material and a preparation method thereof. The coating obtained by laser cladding of the present invention has good macroscopic morphology, the coating and the substrate achieve good metallurgical bonding and has the characteristics of high hardness, high friction and wear resistance, high high temperature oxidation resistance, etc.
[0009] In order to achieve the above technical effects, the present invention is implemented through the following technical solutions: a high entropy alloy material, characterized in that it is composed of four metal element powders of Ti, Mo, Nb, and Cr, each component and its atomic percentage is 16% to 20% Ti, 33% to 38% Mo, 32% to 38% Nb, 17% to 22% Cr, the purity of each component is greater than or equal to 99.9%, and the powder particle size is 150-300 mesh.
[0010] Furthermore, the method for preparing the high entropy alloy material is characterized by comprising the following steps:
[0011] Step 1: Weigh the raw material powders according to the proportion and mix them thoroughly, then add anhydrous ethanol or n-heptane and perform high-energy ball milling to obtain TiMoNbCr high entropy alloy powder;
[0012] Step 2: Pre-treat the base material and polish to remove oxide scale and oil stains;
[0013] Step 3: The TiMoNbCr high entropy alloy powder obtained in Step 1 is pre-placed on the surface of the substrate obtained in Step 2 to form a pre-layer with a thickness of 0.5 to 1.0 mm. The pre-layer is then placed at a constant temperature of 60 to 100°C for 3 to 6 hours, and the cladding layer can be obtained by laser cladding.
[0014] Furthermore, in Step 1, when the added substance is anhydrous ethanol, the high-energy ball milling time is 3 to 5 hours; when the added substance is n-heptane, the ball milling time is 1 to 3 hours.
[0015] Furthermore, the ball mill jar and grinding balls of the high-energy ball mill are made of stainless steel; the ball-to-material ratio is 8:1 to 12:1, and the ball mill rotation speed is 250 r / min to 350 r / min.
[0016] Furthermore, the base material in Step 2 is titanium alloy TC4 (Ti6-A14-V).
[0017] Furthermore, the process parameters of the laser cladding in Step 3 are: laser power 1500-2000 W, scanning speed 600 mm / min, spot diameter 3-5 mm, defocusing amount 20 mm, argon as protective gas, and gas flow rate 8-12 L / min.
[0018] The beneficial effects of the present invention are:
[0019] (1) The TiMoNbCr high entropy alloy material of the present invention is metallurgically bonded to the substrate through laser cladding technology, the substrate and the cladding layer have a high bonding strength, the substrate has a small thermal deformation, a low dilution rate, and a low scrap rate of parts;
[0020] (2) The TiMoNbCr high entropy alloy material of the present invention is to purposefully regulate different components to obtain the expected performance to cope with different working conditions;
[0021] (3) The TiMoNbCr high entropy alloy material in the present invention has a dendrite with uniform structure after laser cladding, and the cladding layer has high hardness, high temperature oxidation resistance and corrosion resistance;
[0022] (4) The laser cladding method has the characteristics of high preparation efficiency (rapid heating and rapid solidification). The thickness of the prepared coating is adjustable and can reach the millimeter level. The instrument operation is relatively simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0024] Figure 1 This is the laser cladding structure diagram of Example 1 of the present invention;
[0025] Figure 2 This is the laser cladding organization diagram of Example 1 of the present invention;
[0026] Figure 3 This is the XRD spectrum of laser cladding in Example 1 of the present invention;
[0027] Figure 4 This is the laser cladding structure diagram of Example 1 of the present invention;
[0028] Figure 5 This is a dendrite composition diagram of laser cladding embodiment 1 of the present invention. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] The high entropy alloy material described in this embodiment is composed of four metal element powders of Ti, Mo, Nb, and Cr. The atomic percentages of each component are 16% Ti, 34% Mo, 32% Nb, and 18% Cr. The sum of the mass percentages of all components is 100%. Each metal powder is weighed using an electronic scale, and the total mass of the mixed powder is 60g.
[0032] The method for preparing the high entropy alloy coating described in this embodiment comprises the following steps:
[0033] (1) After mixing the powders, high-energy ball milling is performed for a ball milling time of not less than 1 hour, and the powders are fully mixed to obtain alloy powders with a powder particle size of 150-300 meshes;
[0034] (2) Grind the base material to remove scale and oil stains;
[0035] (3) The TiMoNbCr high entropy alloy powder obtained in step (1) is pre-placed on the surface of the pre-treated substrate to form a pre-layer with a thickness of 0.5-1.0 mm, and then placed in a constant temperature treatment of 60° C. for 3 hours, and the cladding layer can be obtained by laser cladding. The process parameters for laser cladding are: laser power 2000 W, scanning speed 600 mm / min, spot diameter 5 mm, defocusing amount 20 mm, argon as the protective gas, and gas flow rate 8 L / min.
[0036] In this example, the high entropy alloy cladding layer after laser cladding was polished with high-magnification sandpaper to the metallographic requirements, and photographed and observed with SEM to obtain the organization diagram as shown below: Figure 1 , Figure 2 shown; from Figure 1 , Figure 2 It can be seen that the cladding layer is well bonded to the substrate, and the cladding layer has a dense structure without obvious hole defects.
[0037] The cladding layer is subjected to X-ray diffraction by an X-ray diffractometer (XRD) to obtain the diffraction pattern of the cladding layer, such as Figure 3 As shown; the XRD spectrum shows that the phase structure of the cladding layer is BCC and a small amount of Ti.
[0038] Using EDS spectrometer Figure 4 The composition of the dendrites in Figure 5 As shown in the figure, the primary phases in the dendrites are mainly Ti, Mo, Nb, and Cr, and the high Ti content should be caused by the diffusion of Ti in the matrix.
[0039] The microhardness of the high entropy alloy cladding layer was measured by a microhardness tester. The microhardness of the high entropy alloy cladding layer was measured at different distances from the surface of the cladding layer, and compared with the TiMoNbCr high entropy alloy cladding layer and the base material TC4 steel. The results are shown in the following table. It can be seen from the table that the average hardness value of the TiMoNbCr high entropy alloy cladding layer is 1018HV 0.2 The average hardness of its matrix is 324HV 0.2 Compared with the previous ones, the hardness has been significantly improved.
[0040]
[0041] Example 2
[0042] The high entropy alloy material described in this embodiment is composed of four metal element powders of Ti, Mo, Nb, and Cr. The atomic percentage of each component is 16% Ti, 33% Mo, 32% Nb, and 19% Cr. The sum of the mass percentages of all components is 100%. An electronic scale is used to weigh each metal powder, and the total mass of the mixed powder is 60g.
[0043] The method for preparing the high entropy alloy coating described in this embodiment comprises the following steps:
[0044] (1) After mixing the powders, high-energy ball milling is performed for a ball milling time of not less than 1 hour, and the powders are fully mixed to obtain alloy powders with a powder particle size of 150-300 meshes;
[0045] (2) Grind the base material to remove scale and oil stains;
[0046] (3) The TiMoNbCr high entropy alloy powder obtained in step (1) is pre-placed on the surface of the pre-treated substrate to form a pre-layer with a thickness of 0.5-1.0 mm, and then placed in a constant temperature treatment of 60° C. for 5 hours, and the cladding layer can be obtained by laser cladding. The process parameters for laser cladding are: laser power 1500 W, scanning speed 600 mm / min, spot diameter 3 mm, defocus amount 20 mm, protective gas using argon, and gas flow rate 10 L / min.
[0047] Example 3
[0048] The high entropy alloy material described in this embodiment is composed of four metal element powders of Ti, Mo, Nb, and Cr. The atomic percentage of each component is 16% Ti, 33% Mo, 32% Nb, and 19% Cr. The sum of the mass percentages of all components is 100%. An electronic scale is used to weigh each metal powder, and the total mass of the mixed powder is 60g.
[0049] The method for preparing the high entropy alloy coating described in this embodiment comprises the following steps:
[0050] (1) After mixing the powders, high-energy ball milling is performed for a ball milling time of not less than 1 hour, and the powders are fully mixed to obtain alloy powders with a powder particle size of 150-300 meshes;
[0051] (2) Grind the base material to remove scale and oil stains;
[0052] (3) The TiMoNbCr high entropy alloy powder obtained in step (1) is pre-placed on the surface of the pre-treated substrate to form a pre-layer with a thickness of 0.5-1.0 mm, and then placed in a constant temperature treatment of 100° C. for 5 hours, and the cladding layer can be obtained by laser cladding. The process parameters for laser cladding are: laser power 1500 W, scanning speed 600 mm / min, spot diameter 3 mm, defocusing amount 20 mm, argon as the protective gas, and gas flow rate 10 L / min.
[0053] The high entropy alloy cladding layers after laser cladding prepared in Examples 2 and 3 were polished to the metallographic requirements with high-magnification sandpaper and photographed and observed with SEM. The structures were similar to those in Example 1. The cladding layer was well bonded to the substrate, and the cladding layer had a good microstructure.
[0054] Dense, no obvious hole defects. X-ray diffractometer (XRD) is used to perform X-ray diffraction on the cladding layer. The XRD spectrum shows that the phase structure of the cladding layer is BCC and a small amount of Ti.
Claims
1. A high entropy alloy material, characterized in that: It is composed of four metal element powders of Ti, Mo, Nb and Cr. The atomic percentages of the components are 16% to 20% of Ti, 33% to 38% of Mo, 32% to 38% of Nb, and 17% to 22% of Cr. The purity of each component is greater than or equal to 99.9%, and the powder particle size is 150-300 meshes.
2. A high entropy alloy material according to claim 1, characterized in that: The method for preparing the high entropy alloy material is characterized by comprising the following steps: Step 1: Weigh the raw material powders according to the proportion and mix them thoroughly, then add anhydrous ethanol or n-heptane and perform high-energy ball milling to obtain TiMoNbCr high entropy alloy powder; Step 2: Pre-treat the base material and polish to remove oxide scale and oil stains; Step 3: The TiMoNbCr high entropy alloy powder obtained in Step 1 is pre-placed on the surface of the substrate obtained in Step 2 to form a pre-layer with a thickness of 0.5 to 1.0 mm. The pre-layer is then placed at a constant temperature of 60 to 100°C for 3 to 6 hours, and the cladding layer can be obtained by laser cladding.
3. A high entropy alloy material according to claim 2, characterized in that: In the Step 1, when the added substance is anhydrous ethanol, the high-energy ball milling time is 3 to 5 hours; when the added substance is n-heptane, the ball milling time is 1 to 3 hours.
4. A high entropy alloy material according to claim 2, characterized in that: The ball milling jar and the grinding balls of the high-energy ball mill are made of stainless steel; the ball-to-material ratio is 8:1-12:1, and the ball milling speed is 250r / min-350r / min.
5. A high entropy alloy material according to claim 2, characterized in that: The base material in the Step 2 is titanium alloy TC4 (Ti6-A14-V).
6. A high entropy alloy material according to claim 2, characterized in that: The process parameters of laser cladding in Step 3 are: laser power 1500-2000W, scanning Speed 600mm / min, spot diameter 3-5mm, defocusing amount 20mm, protective gas is argon, Gas flow rate 8~12L / min.