A polypropylene-based insulating material and its preparation method and application
By blending and modifying polypropylene-based autoclave alloy resin with thermoplastic elastomer hydrogenated styrene-butadiene rubber and olefin-based elastomer, the problems of insufficient toughness and poor electrical stability of high-voltage cable insulation materials are solved, achieving higher voltage withstand capabilities. and environmentally friendly recyclability.
Patent Information
- Application Number
- CN202211618685.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-15
AI Technical Summary
The maximum long-term use temperature of existing high-voltage cable insulation materials is about 70°C, which cannot meet the needs of larger-capacity power transmission systems. At the same time, due to insufficient toughness, low breakdown field strength, and poor electrical stability, it is difficult to meet high-voltage needs and cannot be recycled. Cause environmental pollution.
Polypropylene-based kettle alloy resin, thermoplastic elastomer hydrogenated styrene-butadiene rubber and olefin-based elastomer are blended and modified to improve the toughness and electrical stability of the material through the melt blending process, reduce the flexural modulus and enhance the mechanical properties.
It significantly improves the toughness, electrical stability and mechanical properties of the insulating material, meets high voltage requirements, extends the life of the cable, and has the environmental advantage of being recyclable.
Smart Images

Figure CN116041861B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer functional materials, and in particular to a polypropylene-based insulating material and a preparation method and application thereof. Background Art
[0002] At present, high-voltage cables mainly use cross-linked polyethylene as the main insulation material. The maximum long-term operating temperature of the insulated cable is only about 70°C. The cable transmission capacity is limited and cannot meet the use requirements of larger capacity transmission systems. At the same time, the cable cannot be recycled after the life of the cable expires, resulting in a large amount of waste, posing a serious challenge to environmental protection.
[0003] Thermoplastic polypropylene high-voltage cables have the characteristics of high operating temperature and recyclability, becoming a new generation of environmentally friendly cables that can replace cross-linked polyethylene. However, cables made of conventional polypropylene-based insulation materials have many problems such as insufficient toughness, low breakdown field strength, and poor electrical stability, making it difficult to meet the needs of higher voltages. Therefore, it is necessary to further modify polypropylene-based insulation materials to improve their toughness and electrical stability to meet the use and development needs of my country's power grid. Summary of the invention
[0004] Based on this, it is necessary to provide a polypropylene-based insulating material and a preparation method and application thereof that can improve the toughness and electrical stability of the material.
[0005] An embodiment of the present application provides a polypropylene-based insulating material, which includes the following raw materials in parts by weight:
[0006] Polypropylene-based alloy resin in the kettle 30 to 70 parts,
[0007] Thermoplastic elastomer hydrogenated styrene butadiene rubber 10 to 50 parts,
[0008] 10 to 40 parts of olefin-based elastomer.
[0009] In one embodiment, the polypropylene-based in-reactor alloy resin comprises a polypropylene matrix and a toughening phase;
[0010] Optionally, the particle size of the toughening phase is submicron;
[0011] Optionally, the particle size of the toughening phase is 0.4 μm to 1 μm;
[0012] Optionally, the mass content of the toughening phase is 5% to 20%;
[0013] Optionally, the toughening phase comprises ethylene-propylene copolymer;
[0014] Optionally, the polypropylene matrix includes one or more of copolymer polypropylene and homopolypropylene.
[0015] In one embodiment, the thermoplastic elastomer hydrogenated styrene butadiene rubber comprises a hydrogenated styrene-butadiene block copolymer having a number average molecular weight of 150,000 g / mol to 300,000 g / mol.
[0016] In one embodiment, the olefin-based elastomer comprises a propylene-ethylene copolymer elastomer;
[0017] Optionally, in the propylene-ethylene copolymer elastomer, the mass content of ethylene is 8.0% to 12.0%;
[0018] Optionally, the propylene-ethylene copolymer elastomer has a melt index of <2.0 g / 10 min at 230° C. and 2.16 kg.
[0019] In one of the embodiments, the raw material of the polypropylene-based insulation material also includes an antioxidant.
[0020] In one embodiment, the antioxidant is present in an amount of 0.1 to 1.0 parts by weight.
[0021] An embodiment of the present application further provides a method for preparing a polypropylene-based insulating material as described in any of the above embodiments, comprising the following steps:
[0022] The raw materials are provided and melt-blended.
[0023] In one embodiment, the melt blending conditions meet one or more of the following conditions:
[0024] (1) The temperature is 160℃~220℃;
[0025] (2) Duration is 10 to 15 minutes;
[0026] (3) The rotation speed is 60 rpm to 150 rpm.
[0027] In one embodiment, during the melt blending process, the blending method is internal mixing or extrusion.
[0028] An embodiment of the present application also provides a use of the polypropylene-based insulating material as described in any of the above embodiments in the manufacture of cable products.
[0029] The above-mentioned polypropylene-based insulating material uses polypropylene-based in-kettle alloy resin as a base resin, and adds thermoplastic elastomer hydrogenated styrene butadiene rubber and olefin-based elastomer to blend and modify it. The olefin-based elastomer is beneficial to improving the toughness and elasticity of the insulating material and increasing the compatibility between the thermoplastic elastomer hydrogenated styrene butadiene rubber and the base resin; the addition of the thermoplastic elastomer hydrogenated styrene butadiene rubber makes the insulating material have high elasticity, weather resistance and good mechanical properties, can greatly reduce the bending modulus of the insulating material and further improve the toughness of the material, and the raw materials are matched with each other according to specific weight portions, so that the insulating material has excellent toughness and electrical stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 A columnar comparison chart of the bending modulus of the insulating materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4;
[0031] Figure 2 A columnar comparison chart of the breakdown field strength of the insulating materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4;
[0032] Figure 3 This is a bar chart comparison of the oxidation induction time of the insulating materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4. DETAILED DESCRIPTION
[0033] For ease of understanding of the application, the application is described more fully below in conjunction with embodiments and accompanying drawings. The application can be implemented in many different forms and is not limited to the embodiments described in the application. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.
[0034] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more related listed items.
[0035] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0036] In the present application, "plurality", "multiple", "multiple times", "multiples", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0037] The terms "combination thereof", "any combination thereof", "any combination thereof" and the like used in this application include all suitable combinations of any two or more of the listed items.
[0038] In the present application, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc., shall be based on the ability to implement the technical solution of the present invention, solve the technical problem of the present invention, and achieve the expected technical effect of the present invention.
[0039] In the present application, “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects. It should be understood that they do not constitute limitations on the scope of protection of the present invention.
[0040] In the present application, “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.
[0041] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0042] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. For example, therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0043] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0044] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present invention. Specifically, the weight described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0045] An embodiment of the present application provides a polypropylene-based insulating material, which includes the following raw materials in parts by weight:
[0046] Polypropylene-based alloy resin in the kettle 30 to 70 parts,
[0047] Thermoplastic elastomer hydrogenated styrene butadiene rubber 10 to 50 parts,
[0048] 10 to 40 parts of olefin-based elastomer.
[0049] The inventors have found through research that conventional thermoplastic polypropylene resin has poor toughness due to its high glass transition temperature. In addition, conventional polypropylene materials also have many defects such as low breakdown field strength and poor anti-aging performance, which greatly limits the application of polypropylene in cable products, especially high-voltage cables. However, polypropylene-based in-reactor alloy resin can significantly improve the performance limitations of conventional polypropylene resin.
[0050] Polypropylene-based in-kettle alloy resin is a mixed resin composed of polypropylene and other olefin polymers. Other olefin polymers may be, for example but not limited to, rubber polymers such as ethylene-propylene copolymers. The introduction of these rubber polymers can have a toughening effect and is usually called a toughening component or a toughening phase. In addition, compared with conventional polypropylene resins, polypropylene-based in-kettle alloy resins also have significant improvements in properties such as aging resistance.
[0051] In one embodiment, the polypropylene-based autoclave alloy resin includes a polypropylene matrix and a toughening phase.
[0052] Optionally, the particle size of the toughening phase is submicron-sized. The submicron-sized toughening phase particle size is relatively small and can be more evenly dispersed in the polypropylene matrix, so that the properties of the formed polypropylene-based in-reactor alloy resin are more uniform and stable.
[0053] Optionally, the particle size of the toughening phase is 0.4 μm to 1 μm. It is understandable that the particle size of the toughening phase may be, but is not limited to, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, etc.
[0054] Optionally, the mass content of the toughening phase is 5% to 20%. The mass content of the toughening phase within this range can effectively improve the technical effect of improving the toughness of the polypropylene matrix and other properties, while not interfering too much with the original properties of the polypropylene matrix and not affecting the electrical properties of the insulating material. It can be understood that the mass content of the toughening phase can be, for example, but not limited to, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc.
[0055] Alternatively, the toughening phase may include, for example but not limited to, ethylene-propylene copolymer.
[0056] Optionally, the polypropylene matrix may include, for example but not limited to, one or more of copolymer polypropylene and homopolypropylene.
[0057] Thermoplastic elastomer hydrogenated styrene butadiene rubber is an elastomer obtained by selective catalytic hydrogenation of unsaturated carbon-carbon double bonds of styrene butadiene rubber. The inventors found that the thermoplastic elastomer hydrogenated styrene butadiene rubber is used to blend and modify the polypropylene-based in-kettle alloy resin, which can effectively utilize the excellent aging resistance, weather resistance, high elasticity and excellent mechanical properties of the thermoplastic elastomer hydrogenated styrene butadiene rubber, thereby greatly reducing the bending modulus of the insulating material and improving the toughness. While improving the toughness, it can also further improve the comprehensive performance of the insulating material in terms of mechanical strength, aging resistance and dimensional stability.
[0058] In one embodiment, the thermoplastic elastomer hydrogenated styrene butadiene rubber may include, for example but not limited to, a hydrogenated styrene-butadiene block copolymer having a number average molecular weight of 150,000 g / mol to 300,000 g / mol. The hydrogenated styrene-butadiene block copolymer is a linear triblock copolymer, which achieves structural stability mainly through the physical crosslinking points of the styrene segment, wherein the butadiene segment provides softness, has excellent aging resistance, low modulus, high elasticity, good weather resistance and excellent mechanical properties, can effectively improve the elasticity, softness and toughness of the insulating material, can effectively reduce the bending modulus of the insulating material, has excellent electrical properties, thermal properties and mechanical properties, and can also ensure the stability of the insulating material structure.
[0059] Furthermore, the use of hydrogenated styrene-butadiene block copolymers with a molecular weight range of 150,000 g / mol to 300,000 g / mol for blending and modifying polypropylene-based in-vessel alloy resin can significantly improve the aging resistance of the insulating material. It is understandable that the thermoplastic elastomer hydrogenated styrene-butadiene rubber can use a hydrogenated styrene-butadiene block copolymer with a specific molecular weight, or a combination of hydrogenated styrene-butadiene block copolymers with multiple different molecular weights.
[0060] Furthermore, the inventors have also found that introducing a certain amount of olefin-based elastomer into the raw materials of the insulating material can further improve the toughness and elasticity of the insulating material.
[0061] In one embodiment, the olefin-based elastomer may include, for example, but not limited to, propylene-ethylene copolymer elastomer. The propylene-ethylene copolymer elastomer can effectively improve the toughness and elasticity of the polypropylene-based kettle alloy resin. Further, the propylene-ethylene copolymer elastomer can also effectively enhance the compatibility between the toughening phase in the polypropylene-based kettle alloy resin and the polypropylene matrix and the plastic elastomer hydrogenated styrene-butadiene rubber.
[0062] Optionally, in the propylene-ethylene copolymer elastomer, the mass content of ethylene is 8.0% to 12.0%. It is understandable that in the propylene-ethylene copolymer elastomer, the mass content of ethylene can be, for example but not limited to, 8.0%, 8.2%, 8.5%, 8.8%, 9.0%, 9.2%, 9.4%, 9.5%, 9.7%, 9.9%, 10.0%, 10.2%, 10.5%, 10.8%, 11.0%, 11.3%, 11.5%, 11.8%, 12.0%, etc.
[0063] Optionally, the melt index of the propylene-ethylene copolymer elastomer at 230° C. and 2.16 kg is less than 2.0 g / 10 min. The smaller the melt index of the propylene-ethylene copolymer, the more beneficial it is to improve the comprehensive performance of the insulating material in terms of toughness, aging resistance, electrical stability, etc.
[0064] In one embodiment, the raw material of the polypropylene-based insulation material further includes an antioxidant.
[0065] In one embodiment, the antioxidant is present in an amount of 0.1 to 1.0 parts by weight.
[0066] In one embodiment, the antioxidant may be, for example but not limited to, antioxidant 1010 or the like.
[0067] It can be understood that, by weight, 30 to 70 parts of the polypropylene-based alloy resin in the kettle means that the weight of the polypropylene-based alloy resin in the kettle can be, for example but not limited to, 30 parts, 33 parts, 35 parts, 37 parts, 40 parts, 42 parts, 44 parts, 45 parts, 48 parts, 50 parts, 51 parts, 54 parts, 55 parts, 58 parts, 60 parts, 62 parts, 64 parts, 65 parts, 68 parts, 70 parts, etc., and is not limited to this. Any weight value within this range is acceptable.
[0068] It can be understood that, by weight, 10 to 50 parts of the thermoplastic elastomer hydrogenated styrene butadiene rubber means that the weight parts of the thermoplastic elastomer hydrogenated styrene butadiene rubber can be, for example, but not limited to, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, etc., without being limited thereto, and any weight part within this range is acceptable.
[0069] It can be understood that, by weight, 10 to 40 parts of olefin-based elastomer means that the weight of the olefin-based elastomer can be, for example but not limited to, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 23 parts, 25 parts, 26 parts, 28 parts, 30 parts, 31 parts, 33 parts, 35 parts, 36 parts, 38 parts, 39 parts, 40 parts, etc., and is not limited to this. Any weight value within this range is acceptable.
[0070] An embodiment of the present application further provides a method for preparing a polypropylene-based insulating material as in any of the above embodiments, comprising the following steps:
[0071] Various raw materials are provided and melt-blended.
[0072] The melt blending process can greatly improve the dispersibility and compatibility of the raw materials, making the performance of the prepared insulating material more stable.
[0073] In one embodiment, the temperature of melt blending is 160° C. to 220° C. It can be understood that the temperature of melt blending can be, for example but not limited to, 160° C., 165° C., 170° C., 175° C., 180° C., 185° C., 190° C., 195° C., 200° C., 205° C., 210° C., 215° C., 220° C., etc.
[0074] In one embodiment, the time of melt blending is 10 minutes to 15 minutes. It is understandable that the time of melt blending can be, for example but not limited to, 10 minutes, 10.5 minutes, 11 minutes, 11.5 minutes, 12 minutes, 12.5 minutes, 13 minutes, 13.5 minutes, 14 minutes, 14.5 minutes, 15 minutes, etc.
[0075] In one embodiment, the speed of melt blending is 60 rpm to 150 rpm. It is understandable that the speed of melt blending can be, for example, but not limited to, 60 rpm, 65 rpm, 70 rpm, 75 rpm, 80 rpm, 85 rpm, 90 rpm, 95 rpm, 100 rpm, 105 rpm, 110 rpm, 115 rpm, 120 rpm, 125 rpm, 130 rpm, 135 rpm, 140 rpm, 145 rpm, 150 rpm, etc.
[0076] In one embodiment, during the melt blending process, the blending method is internal mixing or extrusion. Internal mixing or extrusion is conducive to improving the dispersibility and compatibility of each raw material, and is helpful to prepare an insulating material with excellent comprehensive performance in terms of toughness, elasticity and electrical stability.
[0077] An embodiment of the present application also provides a use of a polypropylene-based insulating material as in any of the above embodiments in manufacturing a cable product.
[0078] The above-mentioned polypropylene-based insulating material uses polypropylene-based in-kettle alloy resin as a base resin, and adds thermoplastic elastomer hydrogenated styrene butadiene rubber and olefin-based elastomer to blend and modify it. The olefin-based elastomer is beneficial to improving the toughness and elasticity of the insulating material and increasing the compatibility between the thermoplastic elastomer hydrogenated styrene butadiene rubber and the base resin; the addition of the thermoplastic elastomer hydrogenated styrene butadiene rubber makes the insulating material have high elasticity, weather resistance and good mechanical properties, can greatly reduce the bending modulus of the insulating material and further improve the toughness of the material, and the raw materials are matched with each other according to specific weight portions, so that the insulating material has excellent toughness and electrical stability.
[0079] The polypropylene-based insulating material of the present application and its preparation method and application are further described in detail below in combination with specific examples and comparative examples. It can be understood that in the specific examples, unless otherwise specified, all raw materials can be sourced from common commercial sources.
[0080] Among them, the main parameters of some raw material sources are shown in Table 1.
[0081] Table 1 Main parameters of some raw materials
[0082]
[0083] Example 1
[0084] Step 1: Weigh the raw materials
[0085] By weight, 55 parts of polypropylene-based kettle alloy resin, 30 parts of SEBS, 15 parts of propylene-ethylene copolymer elastomer, and 0.5 parts of antioxidant were weighed as raw materials.
[0086] Step 2: Preparation of insulation materials
[0087] The raw materials weighed in step 1 are placed in an internal mixer for melt blending.
[0088] The process conditions of melt blending are: temperature of 180°C, time of 15 minutes, and rotation speed of 90 rpm.
[0089] Example 2
[0090] Step 1: Weigh the raw materials
[0091] By weight, 40 parts of polypropylene-based kettle alloy resin, 20 parts of SEBS, 40 parts of propylene-ethylene copolymer elastomer, and 0.5 parts of antioxidant were weighed as raw materials.
[0092] Step 2: Preparation of insulation materials
[0093] The raw materials weighed in step 1 are placed in an internal mixer for melt blending.
[0094] The process conditions of melt blending are: temperature of 180°C, time of 15 minutes, and rotation speed of 90 rpm.
[0095] Example 3
[0096] Step 1: Weigh the raw materials
[0097] By weight, 60 parts of polypropylene-based kettle alloy resin, 20 parts of SEBS, 20 parts of propylene-ethylene copolymer elastomer, and 0.5 parts of antioxidant were weighed as raw materials.
[0098] Step 2: Preparation of insulation materials
[0099] The raw materials weighed in step 1 are placed in an internal mixer for melt blending.
[0100] The process conditions of melt blending are: temperature of 180°C, time of 15 minutes, and rotation speed of 90 rpm.
[0101] Example 4
[0102] Step 1: Weigh the raw materials
[0103] By weight, 45 parts of polypropylene-based kettle alloy resin, 45 parts of SEBS, 10 parts of propylene-ethylene copolymer elastomer, and 0.5 parts of antioxidant were weighed as raw materials.
[0104] Step 2: Preparation of insulation materials
[0105] The raw materials weighed in step 1 are placed in an internal mixer for melt blending.
[0106] The process conditions of melt blending are: temperature of 180°C, time of 15 minutes, and rotation speed of 90 rpm.
[0107] Comparative Example 1
[0108] Step 1: Weigh the raw materials
[0109] By weight, 65 parts of polypropylene-based kettle alloy resin, 30 parts of SEBS, 5 parts of propylene-ethylene copolymer elastomer, and 0.5 parts of antioxidant were weighed as raw materials.
[0110] Step 2: Preparation of insulation materials
[0111] The raw materials weighed in step 1 are placed in an internal mixer for melt blending.
[0112] The process conditions of melt blending are: temperature of 180°C, time of 15 minutes, and rotation speed of 90 rpm.
[0113] Comparative Example 2
[0114] Step 1: Weigh the raw materials
[0115] By weight, 80 parts of polypropylene-based kettle alloy resin, 20 parts of SEBS, and 0.5 parts of antioxidant were weighed as raw materials.
[0116] Step 2: Preparation of insulation materials
[0117] The raw materials weighed in step 1 are placed in an internal mixer for melt blending.
[0118] The process conditions of melt blending are: temperature of 180°C, time of 15 minutes, and rotation speed of 90 rpm.
[0119] Comparative Example 3
[0120] Step 1: Weigh the raw materials
[0121] By weight, 45 parts of polypropylene-based kettle alloy resin, 10 parts of SEBS, 45 parts of propylene-ethylene copolymer elastomer, and 0.5 parts of antioxidant were weighed as raw materials.
[0122] Step 2: Preparation of insulation materials
[0123] The raw materials weighed in step 1 are placed in an internal mixer for melt blending.
[0124] The process conditions of melt blending are: temperature of 180°C, time of 15 minutes, and rotation speed of 90 rpm.
[0125] Comparative Example 4
[0126] Step 1: Weigh the raw materials
[0127] According to weight, 20 parts of polypropylene-based kettle alloy resin, 80 parts of SEBS and 0.5 parts of antioxidant were weighed as raw materials.
[0128] Step 2: Preparation of insulation materials
[0129] The raw materials weighed in step 1 are placed in an internal mixer for melt blending.
[0130] The process conditions of melt blending are: temperature of 180°C, time of 15 minutes, and rotation speed of 90 rpm.
[0131] The raw materials for preparing the insulating materials of Examples 1 to 4 and Comparative Examples 1 to 4 are listed in Table 2 below.
[0132] Table 2 List of raw materials for the preparation of insulating materials
[0133]
[0134] The flexural modulus, oxidation resistance and electrical properties of the insulating materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were tested, and the test results are shown in Table 3. The test method is:
[0135] The bending modulus is tested based on GB / T9341-2008; the bending modulus of the insulating materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4 is as follows: Figure 1 shown.
[0136] The electrical properties are tested based on GB / T 1408.1-2016; the breakdown field strength of the insulating materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4 is as follows: Figure 2 shown.
[0137] Antioxidation performance Using a differential scanning calorimeter (TAQ250), 5 mg of the sample was placed in an open crucible, and the temperature was raised from room temperature to 210°C at a heating rate of 20°C / min in a nitrogen atmosphere, and the temperature was kept constant for 3 minutes; then, the sample heat flow signal was detected in an oxygen atmosphere to calculate the oxidation induction time. The oxidation induction time of the insulating materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4 is shown in Figure 3 shown.
[0138] Table 3 Performance test results of insulation materials
[0139]
[0140] Depend on Figure 1 to Figure 3 As can be seen from the results in Table 3, the insulating materials prepared in Examples 1 to 4 have suitable bending modulus, good toughness, high breakdown field strength, good electrical stability, oxidation induction time within a suitable range, and good aging resistance.
[0141] The flexural modulus of the insulating materials prepared in Comparative Examples 1 and 2 is too high, the material toughness is poor, and the breakdown field strength of Comparative Example 1 decreases significantly, and the electrical stability is poor.
[0142] The insulating material prepared in Comparative Example 3 has too low breakdown field strength and poor electrical stability.
[0143] The flexural modulus of the insulating material prepared in Comparative Example 4 is too low and the rigidity is insufficient, which affects the long-term creep resistance.
[0144] The technical features of the above embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0145] The above embodiments only express several embodiments of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the inventive concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A polypropylene-based insulating material, characterized in that: The following raw materials are included by weight: 40 to 60 parts of polypropylene-based alloy resin in the kettle, Thermoplastic elastomer hydrogenated styrene butadiene rubber 20 to 45 parts, 10 to 40 parts of olefin-based elastomer; The polypropylene-based in-kettle alloy resin comprises a polypropylene matrix and a toughening phase, the particle size of the toughening phase is submicron-level, and the mass content of the toughening phase is 5% to 20%; The olefin-based elastomer includes a propylene-ethylene copolymer elastomer.
2. The polypropylene-based insulating material according to claim 1, characterized in that: The particle size of the toughening phase is 0.4 μm to 1 μm.
3. The polypropylene-based insulating material according to claim 1, characterized in that: The toughening phase includes ethylene-propylene copolymer.
4. The polypropylene-based insulating material according to claim 1, characterized in that: The polypropylene matrix includes one or more of copolymer polypropylene and homopolypropylene.
5. The polypropylene-based insulating material according to claim 1, characterized in that: The thermoplastic elastomer hydrogenated styrene butadiene rubber comprises a hydrogenated styrene-butadiene block copolymer with a number average molecular weight of 150000 g / mol to 300000 g / mol.
6. The polypropylene-based insulating material according to claim 1, characterized in that: The mass content of ethylene in the propylene-ethylene copolymer elastomer is 8.0% to 12.0%.
7. The polypropylene-based insulating material according to claim 6, characterized in that: The propylene-ethylene copolymer elastomer has a melt index of less than 2.0 g / 10 min at 230° C. and 2.16 kg.
8. The polypropylene-based insulating material according to any one of claims 1 to 7, characterized in that: The raw materials of the polypropylene-based insulating material also include an antioxidant.
9. The polypropylene-based insulating material according to claim 8, characterized in that: In terms of weight, the antioxidant is 0.1 to 1.0 parts.
10. A method for preparing a polypropylene-based insulating material according to any one of claims 1 to 9, characterized in that: The steps include: The raw materials are provided and melt-blended.
11. The method for preparing a polypropylene-based insulating material according to claim 10, characterized in that: The conditions for melt blending meet one or more of the following conditions: (1) The temperature is 160℃~220℃; (2) Duration is 10 to 15 minutes; (3) The rotation speed is 60 rpm to 150 rpm.
12. The method for preparing a polypropylene-based insulating material according to claim 11, characterized in that: In the process of melt blending, the blending method is internal mixing or extrusion.
13. Use of the polypropylene-based insulating material according to any one of claims 1 to 9 in the manufacture of cable products.