A kind of spandex fiber with improved unwinding property and preparation method thereof

By adding cyclotriteratos and its derivatives as unwinding improvement aids to spandex fiber, and combining it with dry spinning technology, the problem of poor unwinding properties of spandex fiber caused by long storage time has been solved, and the unwinding improvement in spandex fiber has been achieved. Maintain good unwinding properties and mechanical properties during storage.

CN116043359BActive Publication Date: 2024-10-01ZHEJIANG HUAFENG SPANDEX
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310156042.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-23
Publication Date
2024-10-01
Estimated Expiration
2043-02-23

AI Technical Summary

Technical Problem

The existing technology cannot effectively solve the problem of poor unwinding properties of spandex fiber due to long storage time.

Method used

Add 0.3% to 5% unwinding improvement additives to the spandex fiber, including cyclotriterrestrial hydrocarbon and its derivatives, and dry-spinning after mixing with the polyurethane-urea solution, and coating with spinning oil to improve Unwindability.

Benefits of technology

It effectively improves the problem of deterioration of unwinding properties of spandex fibers caused by long storage time, and has no impact on mechanical properties. It maintains good unwinding properties after laboratory simulated aging accelerated experiments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004092374850000031
    Figure BDA0004092374850000031
  • Figure BDA0004092374850000041
    Figure BDA0004092374850000041
  • Figure BDA0004092374850000071
    Figure BDA0004092374850000071
Patent Text Reader

Abstract

The invention discloses a spandex fiber with improved unwinding property and a preparation method thereof. The spandex fiber with improved unwinding property contains 0.3% to 5% of an unwinding improving agent calculated based on the mass of the spandex fiber, and the unwinding improving agent comprises cyclotriveratrol and its derivatives. The preparation method comprises the following steps: mixing the unwinding agent with a polyurethane-urea solution, and then using the polyurethane-urea solution containing the unwinding improving agent as a spinning stock solution after aging to obtain the fiber through dry spinning; the polyurethane-urea solution comprises a polyurethane prepolymer mixed amine and reacts to obtain the fiber. The invention effectively improves the problem of deterioration of the unwinding property of the spandex fiber caused by long storage time by adding the unwinding improving agent containing a lipophilic cavity structure into the spandex fiber, and the spandex fiber to which the unwinding improving agent is added has no influence on its mechanical properties, and can maintain good unwinding property after a laboratory simulated aging accelerated test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a spandex fiber with improved unwinding performance and a preparation method thereof, belonging to the technical field of polyurethane elastic fibers. Background Art

[0002] Spandex is the abbreviation of polyurethane elastic fiber (Polyurethane), which is a polyurethane elastic fiber containing more than 85% carbamate groups and having a linear molecular chain structure. Spandex fiber has special properties such as high elongation at break (400% to 800%) and high elastic recovery rate (up to 95% recovery rate after 300% elongation), so it is widely used in elastic fabrics and expanded to medical, sports and other fields. At present, spandex fiber undergoes an oiling process during production to give it better unwinding properties and facilitate subsequent processing and use. However, after the production of spandex fiber, it needs to be stored and transported, especially cross-border transportation, which takes several months. It also needs to be stored when used by customers. In addition, the storage conditions at customers are generally poor and the temperature is high, which causes the surface oil of spandex yarn to volatilize. When customers weave, the silk rolls are not easy to unwind, and it is easy to have broken silk and other faults, which affects the subsequent use.

[0003] Conventional methods for improving the unwinding properties of spandex fibers can only improve the unwinding properties of spandex when it is just produced, and the initial unwinding properties of spandex fibers also have an upper limit due to various factors. For example, the commonly used methods are to add lubricant magnesium stearate to spandex fibers and to increase the oil content of spandex fibers. Excessive lubricant content in spandex fibers will lead to problems such as poor forming of spandex finished products and low cohesion, affecting customer use. The surface oil of spandex fibers exists by physical adsorption. The thickness of the oil film on the fiber surface limits the upper limit of the oil content. Excessive oil content will also lead to problems such as uneven ends of the silk cakes, railway tracks, and falling edges. Excessive oil film thickness also means that it is more volatile and cannot adhere to the fiber surface for a long time. Therefore, conventional methods for improving unwinding properties cannot solve the problem of poor unwinding properties of spandex fibers due to long storage time.

[0004] Patent CN110923844A discloses a method for preparing spandex that is easy to unwind, which is to use a polyurethane stock solution of a polytetramethylene ether glycol system and an alkali-soluble polyester to blend and spin, then soak in a high-temperature alkali solution pool at 80-100°C for 30-300s, dry with hot air at 40-70°C, cool for 10-30°C, set for 10-300s, and then oil to obtain spandex that is easy to unwind. However, after alkali treatment, the physical properties of the spandex will be greatly reduced, and the method is complex in process and high in production cost, and cannot be promoted and applied.

[0005] Patent CN102704034A discloses a method for preparing spandex fiber suitable for high-speed unwinding. The method is to add a relaxant magnesium stearate to a polymer, the mass content of magnesium stearate in the polymer is 0.1-1.5%, and the particle size of magnesium stearate is 0.3-5μm; in the oiling process, the oil agent is selected as silicone oil, magnesium stearate is added to the silicone oil, the mass percentage of magnesium stearate is 0.5-1.5%, and the oiling rate is 4-6%, thereby improving the unwinding property of fine denier spandex. Patent CN107502978A discloses a spandex for diapers with improved unwinding property and creep property and a production method thereof. The method is to add thermoplastic polyurethane, tackifier and lubricant to polyurethane urea stock solution, and use dry spinning technology to improve the unwinding property and creep property of spandex. This method also cannot solve the problem of deterioration of unwinding property of spandex fiber due to long storage time. Patent CN113005559A discloses a method for preparing nano-modified easy-to-unwind spandex, which uses highly dispersible nano-lubricating materials as lubricating additives for spandex, solving the problems of broken yarns and adhesion during unwinding of spandex in downstream applications. Although the above patents have the effect of improving the unwinding properties of spandex fibers, they cannot solve the problem of deterioration of the unwinding properties of spandex fibers caused by long storage time. Summary of the invention

[0006] Technical problem: In order to overcome the problems existing in the background technology, the present invention provides a spandex fiber with improved unwinding property and a preparation method thereof, which is used to solve the problem of deterioration of the unwinding property of the spandex fiber due to long storage time.

[0007] Technical solution: The present invention provides a spandex fiber with improved unwinding properties. The spandex fiber contains 0.3% to 5% of an unwinding improving agent based on the mass of the spandex fiber. The unwinding improving agent includes cyclotriveratrol and its derivatives.

[0008] The cyclotriveratrol contains a cavity structure, including at least one of cap-type cavernous cyclotriveratrol and cavean.

[0009] The cap-type cryptal cyclotriveratrol includes one or more of quasi-cryptal 1, quasi-cryptal 2, quasi-cryptal 3 and quasi-cryptal 4.

[0010] The cryptophane comprises one or more of Cryptophane-A, Cryptophane-E and Cryptophane-O.

[0011] The preparation method of the spandex fiber with improved unwinding property of the present invention comprises the following steps: mixing an unwinding aid with a polyurethane-urea solution, and then using the polyurethane-urea solution containing the unwinding improvement aid to prepare a spinning solution through dry spinning;

[0012] The polyurethane-urea solution is obtained by reacting a polyurethane prepolymer and a mixed amine;

[0013] The spandex fiber is coated with a spinning oil; the spinning oil accounts for 0.1 to 6% of the fiber mass;

[0014] The polyurethane prepolymer comprises an NCO-terminated polyurethane prepolymer obtained by reacting a polyhydroxy polymer and a polyisocyanate, wherein the NCO mass content of the polyurethane prepolymer is 2-4%; the polyhydroxy polymer comprises a polyether diol and / or a polyester diol; and the number average molecular weight of the polyhydroxy polymer is 1000-4000.

[0015] The polyether diols include at least one of polyoxyethylene ether diol, polyoxypropylene ether diol and polytetramethylene ether diol; the polyester diols include at least one of polyethylene adipate diol, polybutylene adipate diol, polyhexamethylene adipate diol and polycaprolactone diol.

[0016] The polyisocyanate includes one or more of diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate and / or derivatives and / or modified polymers;

[0017] The mixed amines include small molecule monoamines and small molecule diamines; the small molecule monoamines include one or more of ethylamine, n-propylamine, isopropylamine, n-butylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, di-n-butylamine, and cyclohexylamine; the small molecule diamines include one or more of ethylenediamine, propylenediamine, 2-methyl-1,5-pentanediamine, cyclohexanediamine, and trimethylhexamethylenediamine.

[0018] Beneficial effect: The present invention effectively improves the problem of deterioration of the unwinding property of the spandex fiber caused by long storage time by adding an unwinding improvement aid containing a lipophilic cavity structure into the spandex fiber. The spandex fiber to which the unwinding aid is added has no effect on its mechanical properties, and can maintain good unwinding property after laboratory simulated aging accelerated test. DETAILED DESCRIPTION

[0019] The spandex fiber contains 0.3% to 5% of an unwinding improvement agent, calculated based on the weight of the spandex fiber, and the unwinding improvement agent includes cyclotriveratrol and its derivatives;

[0020] The cyclotriveratrol contains a cavity structure, including at least one of cap-shaped cryptal cyclotriveratrol and cryptal;

[0021] Furthermore, the cap-type cryptate cyclotriveratrol includes one or more of quasi-cryptate 1, quasi-cryptate 2, quasi-cryptate 3, and quasi-cryptate 4;

[0022] As an example, the cap-type cryptate-shaped cyclotriveratrol structure is as follows:

[0023]

[0024] Furthermore, the cryptophane comprises one or more of Cryptophane-A, Cryptophane-E, and Cryptophane-O;

[0025] As an example, the hole fan structure is as follows:

[0026]

[0027] The method for preparing the spandex fiber with improved unwinding property comprises: using a polyurethane-urea solution containing an unwinding improving auxiliary agent as a spinning solution and obtaining the spandex fiber by dry spinning;

[0028] Furthermore, the spandex fiber is coated with a spinning oil, and the spinning oil can be a commonly used oil in the art;

[0029] As an example, the oils include WHF-9018, NF-3, DY-1033, RZ-3209F

[0030] Furthermore, the polyurethane-urea solution is dry-spun after being aged;

[0031] Preferably, the polyurethane-urea solution comprises a polyurethane prepolymer mixed with an amine and obtained by reacting;

[0032] The polyurethane prepolymer comprises a polyol polymer and a polyisocyanate to obtain an NCO-terminated polyurethane prepolymer;

[0033] The NCO mass content of the polyurethane prepolymer is 2-4%;

[0034] The polyhydroxy polymer includes polyether diol and / or polyester diol;

[0035] Preferably, the number average molecular weight of the polyhydroxy polymer is 1000 to 4000;

[0036] The polyether diol includes one or more of polyoxyethylene ether diol, polyoxypropylene ether diol and polytetramethylene ether diol;

[0037] The polyester diol includes one or more of polyethylene adipate diol, polybutylene adipate diol, polyhexamethylene adipate diol and polycaprolactone diol;

[0038] The polyisocyanate includes one or more of diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate and / or derivatives and / or modified polymers;

[0039] The mixed amine includes small molecule monoamine and small molecule diamine;

[0040] The small molecule monoamine includes one or more of ethylamine, n-propylamine, isopropylamine, n-butylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, di-n-butylamine, and cyclohexylamine;

[0041] The small molecule diamine includes one or more of ethylenediamine, propylenediamine, 2-methyl-1,5-pentanediamine, cyclohexanediamine, and trimethylhexamethylenediamine.

[0042] The molar ratio of the total amine groups of the end capping agent and the chain extender to the NCO of the polyurethane prepolymer is 1.0 to 1.1, preferably 1.05 to 1.08;

[0043] In some embodiments of the present invention, the method for preparing the spandex fiber with improved unwinding property comprises:

[0044] In the presence of a solvent, a polyurethane prepolymer and a mixed amine are reacted to obtain a polyurethane-urea polymer solution; after an unwinding improving auxiliary agent is added to the polyurethane-urea polymer solution and the solution is aged, the solution is prepared by dry spinning;

[0045] The solvent is N,N-dimethylformamide and / or N,N-dimethylacetamide.

[0046] Furthermore, the spandex fiber prepared by dry spinning is dried, oiled, and wound to obtain a spandex fiber cake with an oil agent coated on the surface.

[0047] As an example, the method for preparing the spandex fiber with improved unwinding property comprises the following steps:

[0048] Preparation of polyurethane prepolymer: react polyhydroxy polymer and polyisocyanate at a temperature of 50 to 100° C. for 2 to 5 hours to obtain polyurethane prepolymer;

[0049] Preferably, the reaction temperature is 70-80° C. and the reaction time is 3-4 h.

[0050] Preparation of polyurethane-urea polymer solution: fully dissolving polyurethane prepolymer to obtain prepolymer solution, mixing with mixed amine solution to obtain polyurethane-urea polymer solution, the reaction temperature is 6-15° C., and the reaction time is 1-2 hours;

[0051] Preferably, the reaction temperature is 6 to 15°C and the reaction time is 1.2 to 1.5h;

[0052] The mass percentage of the prepolymer solution is 33% to 55%, and the mass percentage of the mixed amine is 4% to 5%.

[0053] Preparation of spinning solution: adding an unwinding improving agent to a polyurethane-urea polymer solution, and aging at a temperature of 40 to 50° C. for 30 to 40 hours to obtain a spinning solution;

[0054] Wherein, the mass percentage of the spinning solution is 30% to 45%;

[0055] Preferably, conventional additives in the field can be added to the spinning solution. For example, the additives can include dispersants, antioxidants, lubricants, matting agents, ultraviolet absorbers, etc. There is no special requirement for the amount of additives added as long as the performance of the spandex fiber itself is not affected.

[0056] Aging spinning step: the spinning solution is subjected to dry spinning technology through steps including spraying, stretching and high-temperature drying to obtain fibers, and then through steps such as oiling with an oil agent and winding and forming to obtain spandex fibers with improved unwinding properties.

[0057] Preferably, the spinning oil is selected from RZ-3209F and DY-1033, and the spinning oil coated on the surface of the spandex fiber accounts for 0.1-6% of the fiber mass.

[0058] The specific operation process of the present invention is described in detail below with specific examples, but these examples should not be understood as limiting the present invention in any sense.

[0059] Preparation of polyurethane prepolymer: polytetramethylene ether glycol and diphenylmethane diisocyanate were reacted at 80°C for 4 hours to obtain a polyurethane prepolymer with an NCO mass content of 2.6%;

[0060] Preparation of polyurethane-urea polymer solution: fully dissolving polyurethane prepolymer in N,N-dimethylacetamide to obtain prepolymer solution, and mixing with mixed amine solution containing ethylenediamine, propylenediamine and diethylamine to obtain polyurethane-urea polymer solution, the reaction temperature is 8°C, and the reaction time is 1.25h;

[0061] The mass percentage of the prepolymer solution is 40%, and the mass percentage of the mixed amine is 4.5%.

[0062] Example 1

[0063] The spandex fiber contains 2.5% of Cryptophane-E unwinding improvement auxiliary agent, and based on the weight of the spandex fiber, the spandex fiber is coated with 3% of spinning oil RZ-3209F.

[0064] Example 2

[0065] The spandex fiber contains 3% of the unwinding improvement auxiliary agent of quasi-xuefan 2, and the spandex fiber is coated with 3% of the spinning oil RZ-3209F based on the mass of the spandex fiber.

[0066] Example 3

[0067] The spandex fiber contains 5% of the unwinding improvement auxiliary agent RZ-3209F, and is coated with 3% of the spinning oil RZ-3209F based on the weight of the spandex fiber.

[0068] Example 4

[0069] The spandex fiber contains 0.3% of Cryptophane-A unwinding improvement auxiliary agent, and based on the weight of the spandex fiber, the spandex fiber is coated with 3% of the spinning oil RZ-3209F.

[0070] Example 5

[0071] The spandex fiber contains 2.5% of a crown-type cyclotriveratrol unwinding improving auxiliary agent, and based on the weight of the spandex fiber, the spandex fiber is coated with 3% of a spinning oil RZ-3209F.

[0072] Example 6

[0073] The spandex fiber contains 2.5% of cyclodextrin unwinding improvement auxiliary agent, and based on the weight of the spandex fiber, the spandex fiber is coated with 3% of spinning oil RZ-3209F.

[0074] Comparative Example 1

[0075] The spandex fiber contains 2.5% of magnesium stearate unwinding improvement auxiliary agent, and based on the weight of the spandex fiber, the spandex fiber is coated with 3% of spinning oil RZ-3209F.

[0076] Comparative Example 2

[0077] The spandex fiber contains 2.5% of magnesium stearate unwinding improvement auxiliary agent, and based on the weight of the spandex fiber, the spandex fiber is coated with 6% of spinning oil RZ-3209F.

[0078] Comparative Example 3

[0079] The spandex fiber does not contain an unwinding improving auxiliary agent, and the spandex fiber is coated with 6% of a spinning oil RZ-3209F.

[0080] Comparative Example 4

[0081] The spandex fiber does not contain an unwinding improving auxiliary agent, and the spandex fiber is coated with 10% of a spinning oil RZ-3209F.

[0082] The above embodiments are merely descriptions of preferred implementations of the present invention, and are not intended to limit the present invention. Without departing from the design spirit of the present invention, various improvements made to the technical solutions of the present invention by ordinary technicians in the field should fall within the protection scope of the present invention.

[0083] The 44dtex spandex fiber prepared according to the embodiment of the present invention and the comparative example were tested for mechanical properties and unwinding properties, respectively. It can be found that the mechanical properties of the spandex fiber prepared in the embodiment of the present invention are not significantly different from those of the comparative example. However, after the laboratory simulated accelerated aging experiment, the unwinding property is significantly better than that of the comparative example. The specific test data are compared in Tables 1 and 2.

[0084] Performance test of spandex fiber:

[0085] (1) Mechanical properties: The spandex fiber was tested using a constant-rate tensile strength testing machine. The breaking strength, breaking elongation, and strength at 300% elongation were tested under specified length and pre-tension.

[0086] (2) Laboratory simulated accelerated aging experiment: The spandex fiber is placed in an electric hot air drying oven, the temperature is adjusted to 60°C, and the constant temperature is dried for 72 hours, and then the unwinding test is performed. The smaller the unwinding test data, the better the unwinding performance.

[0087] Table 1: Mechanical properties test data of the embodiments of the present invention and the comparative examples

[0088]

[0089] Table 2: Unwinding test data of the embodiments of the present invention and the comparative examples

[0090]

Claims

1. A spandex fiber with improved unwinding properties, characterized in that: The spandex fiber contains 0.3% to 5% of an unwinding improvement agent based on the spandex fiber mass, and the unwinding improvement agent includes cyclotriveratrol. ; The cyclotriveratrol contains a cavity structure, including at least one of cap-type cavernous cyclotriveratrol and cavean.

2. The spandex fiber with improved unwinding property according to claim 1, characterized in that: The cap-type cryptate cyclotriveratrol includes one or more of quasi-cryptate 1, quasi-cryptate 2, quasi-cryptate 3, and quasi-cryptate 4; 3. The spandex fiber with improved unwinding property according to claim 1, characterized in that: The cryptophane comprises one or more of Cryptophane-A, Cryptophane-E and Cryptophane-O.

4. A method for preparing a spandex fiber with improved unwinding properties as claimed in claim 1, characterized in that: The method comprises mixing an unwinding aid with a polyurethane-urea solution, and then using the polyurethane-urea solution containing the unwinding aid to cure the solution to obtain a spinning solution by dry spinning; The polyurethane-urea solution is obtained by reacting a polyurethane prepolymer with a mixed amine.

5. The method for preparing the spandex fiber with improved unwinding property according to claim 4, characterized in that: The spandex fiber is coated with a spinning oil; the spinning oil accounts for 0.1-6% of the fiber mass.

6. The method for preparing the spandex fiber with improved unwinding property according to claim 4, characterized in that: The polyurethane prepolymer comprises an NCO-terminated polyurethane prepolymer obtained by reacting a polyhydroxy polymer and a polyisocyanate, wherein the NCO mass content of the polyurethane prepolymer is 2-4%; the polyhydroxy polymer comprises a polyether diol and / or a polyester diol; and the number average molecular weight of the polyhydroxy polymer is 1000-4000.

7. The method for preparing the spandex fiber with improved unwinding property according to claim 6, characterized in that: The polyether diols include at least one of polyoxyethylene ether diol, polyoxypropylene ether diol and polytetramethylene ether diol; the polyester diols include at least one of polyethylene adipate diol, polybutylene adipate diol, polyhexamethylene adipate diol and polycaprolactone diol.

8. The method for preparing spandex fiber with improved unwinding property according to claim 6, characterized in that: The polyisocyanate includes one or more of diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate and / or derivatives and / or modified polymers.

9. The method for preparing spandex fiber with improved unwinding property according to claim 4, characterized in that: The mixed amines include small molecule monoamines and small molecule diamines; the small molecule monoamines include one or more of ethylamine, n-propylamine, isopropylamine, n-butylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, di-n-butylamine, and cyclohexylamine; the small molecule diamines include one or more of ethylenediamine, propylenediamine, 2-methyl-1,5-pentanediamine, cyclohexanediamine, and trimethylhexamethylenediamine.