Polytetrafluoroethylene composite and porous membrane thereof and preparation method and application thereof

By using the mixing of polytetrafluoroethylene resins of different densities and co-extrusion agents and a specific process, a polytetrafluoroethylene porous membrane with high filtration efficiency and good air permeability is prepared, which solves the problem of barrier efficiency and air permeability in the existing technology. A matter of balance.

CN116059849BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111281846.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-01
Publication Date
2024-10-15
Estimated Expiration
2041-11-01

AI Technical Summary

Technical Problem

While the existing polytetrafluoroethylene porous membrane improves the barrier efficiency, its air permeability will be lost, making it difficult to combine high barrier efficiency and good air permeability.

Method used

Two polytetrafluoroethylene resins and extrusion aids with different relative standard densities are used to mix, and through specific pressure conditions and stretching processes, a polytetrafluoroethylene porous membrane with composite characteristics is prepared to ensure high filtration efficiency and Taking into account breathability.

Benefits of technology

It achieves the high salt media filtration efficiency and good air permeability of the polytetrafluoroethylene porous membrane. The product's salt media filtration efficiency is not less than 95%, the air permeability is around 3L/min, and it has the high barrier efficiency and breathability of the composite structure. Advantages of good sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116059849B_ABST
    Figure CN116059849B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of polytetrafluoroethylene filter materials, and discloses a polytetrafluoroethylene composite, a porous membrane, and a preparation method and application thereof. The polytetrafluoroethylene composite comprises component A, component B, and component C; both component A and component B are polytetrafluoroethylene resins, and the average relative standard density of component A is greater than the average relative standard density of component B; component C is an extrusion aid. The polytetrafluoroethylene porous membrane provided by the present invention has composite characteristics, not only has high barrier efficiency, but also has good air permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polytetrafluoroethylene filter materials, and more particularly to a polytetrafluoroethylene composite, a porous membrane, and a preparation method and application thereof. Background Art

[0002] Polytetrafluoroethylene porous membrane has the advantages of high tensile strength, large specific surface area, high porosity, good air permeability, high inertness, non-toxicity and non-allergenic side effects, and is widely used in defense, aerospace, petrochemical, clothing, medical and health fields. In the field of medical and health, polytetrafluoroethylene porous membrane has the advantages of highly stable high filtration efficiency, waterproof and breathable, washable and reusable, aging resistance, etc., and is widely used in medical masks, reusable protective clothing, surgical gowns, etc., especially suitable as strategic materials that need to be preserved for a long time. In the face of large-scale epidemics, the disadvantages of traditional disposable medical protection products are highlighted. For example, the shelf life of disposable surgical masks is less than two years, and the attenuation of static electricity on the mask will greatly reduce its filtration performance, which is not suitable for strategic reserves. In the face of sudden large-scale demand, it is difficult to meet the demand with production capacity. At the same time, disposable medical textiles that have been used in large quantities can only be incinerated, which brings serious environmental problems. Disposable medical protective equipment and reusable medical protective equipment will coexist for a long time. Reusable medical protective equipment has more advantages in responding to large-scale public health crises. Polytetrafluoroethylene porous membrane is such a material that can meet the requirements of long-term preservation and reusability.

[0003] At present, the biaxial stretching method is the main method for preparing polytetrafluoroethylene porous membranes. The microporous membranes prepared by this method have the advantages of small and uniform pore size distribution and high porosity. In the 1970s, Gore Company in the United States first used the biaxial stretching method to prepare polytetrafluoroethylene porous membranes, and it has been used to this day. Its process flow is: PTFE resin, extrusion aid → mixing → preforming → pushing → calendering → biaxial stretching → heat setting treatment, through longitudinal and transverse stretching, and then heat setting treatment to finally obtain film products. After biaxial stretching, polytetrafluoroethylene forms a multi-microporous structure formed by microfibrils connected to nodes, with a pore size between 0.1-10μm, a porosity of more than 80%, and has a wide operating temperature range (-200℃-260℃), a small friction coefficient, stable chemical properties, and low surface energy. The polytetrafluoroethylene porous membrane relies on pure physical interception to achieve efficient filtration. While improving the interception efficiency, its air permeability will be lost. Especially in the case of high barrier efficiency, it cannot have both high barrier efficiency and good air permeability.

[0004] At present, providing a polytetrafluoroethylene porous membrane with both good barrier efficiency and air permeability is a technical problem that needs to be solved. Summary of the invention

[0005] In view of the above technical problems, the present invention provides a polytetrafluoroethylene composite, a porous membrane and a preparation method and application thereof. The polytetrafluoroethylene porous membrane provided by the present invention has composite characteristics, not only has high barrier efficiency, but also has good air permeability.

[0006] One of the purposes of the present invention is to provide a polytetrafluoroethylene composite, comprising component A, component B and component C; the component A and component B are both polytetrafluoroethylene resins, the average relative standard density of the component A is greater than the average relative standard density of the component B; and component C is an extrusion aid.

[0007] In a preferred embodiment of the present invention, the average relative standard density of component A and component B is respectively 2.1-2.2 g / cm 3 between.

[0008] In a preferred embodiment of the present invention, the average relative standard density of component A is 2.161-2.2 g / cm 3 .

[0009] In a preferred embodiment of the present invention, the average relative standard density of component B is 2.13-2.160 g / cm 3 .

[0010] In a preferred embodiment of the present invention, the thermal instability coefficients of component A and component B are each no greater than 50.

[0011] According to the present invention, the selection range of the ratio is relatively wide. In a preferred embodiment of the present invention, in terms of weight percentage, relative to the total weight of the polytetrafluoroethylene composite, the content of component A is 5-90 weight%, the content of component B is 5-90 weight%, and the content of component C is 5-50 weight%. More preferably, relative to the total weight of the polytetrafluoroethylene composite, the content of component A is 10-50 weight%, the content of component B is 30-70 weight%, and the content of component C is 5-30 weight%.

[0012] According to the present invention, in terms of weight percentage, relative to the total weight of the polytetrafluoroethylene composite, the content of component A is 5-90 weight %, preferably 10-50 weight %, for example, 10 weight %, 20 weight %, 30 weight %, 40 weight %, 50 weight %, and any value between 10 weight % and 50 weight % and any interval between any two values.

[0013] According to the present invention, in terms of weight percentage, relative to the total weight of the polytetrafluoroethylene composite, the content of component B is 5-90 weight%, preferably 30-70 weight%, for example, 30 weight%, 40 weight%, 50 weight%, 60 weight%, 70 weight%, and any value between 30 weight% and 70 weight% and any interval between any two values.

[0014] According to the present invention, in terms of weight percentage, relative to the total weight of the polytetrafluoroethylene composite, the content of component C is 5-50 weight%, preferably 5-30 weight%, for example, 5 weight%, 10 weight%, 15 weight%, 20 weight%, 25 weight%, 30 weight%, any value between 5 weight% and 30 weight% and any interval between any two values.

[0015] In a preferred embodiment of the present invention, the component A and the component B are independently selected from polytetrafluoroethylene resins obtained by dispersion polymerization.

[0016] The component C can be selected from a variety of options. In a preferred embodiment of the present invention, the component C is selected from at least two of aviation kerosene, white oil, naphtha, isoparaffins and kerosene; preferably, the component C is selected from at least two of aviation kerosene, white oil and isoparaffins. More preferably, the component C is selected from aviation kerosene and isoparaffins, and based on the total weight of the component C being 100%, the content of the aviation kerosene is 10-50% by weight, and the content of the isoparaffins is 50-90% by weight.

[0017] The second object of the present invention is to provide a method for preparing a polytetrafluoroethylene composite porous membrane, comprising mixing the components including the component A, the component B and the component C.

[0018] In a preferred embodiment of the present invention, the mixing is performed under pressure, preferably, the mixing pressure is 0.2-10 MPa; and / or, the mixing time is 10-150 h.

[0019] In a preferred embodiment of the present invention, the mixing method is non-stirring mixing, preferably rotating the container to drive the materials in the container to mix, and the preferred rotation speed is 10-200 rpm.

[0020] In a preferred embodiment of the present invention, the mixing includes standing, preferably, the standing time is 10-20 hours; and / or the standing temperature is 40-80°C.

[0021] The third object of the present invention is to provide a polytetrafluoroethylene composite porous membrane, which is made of the polytetrafluoroethylene composite material described above.

[0022] In a preferred embodiment of the present invention, the salt medium filtration efficiency of the polytetrafluoroethylene composite porous membrane is not less than 95%; and / or, at a pressure of 7 kPa and a test area of ​​20 cm 2 The air permeability under the conditions is 2-10 L / min, preferably 2-5 L / min.

[0023] A fourth object of the present invention is to provide a method for preparing the polytetrafluoroethylene composite porous membrane as described above, comprising forming a membrane from the polytetrafluoroethylene composite; preferably, comprising preforming, pushing and extruding, calendering, biaxially stretching, heat setting, and then cooling the polytetrafluoroethylene composite.

[0024] In a more preferred embodiment of the present invention, the raw materials of the polytetrafluoroethylene compound described above are mixed under pressure, then allowed to stand, and then preformed, pushed and extruded, calendered, synchronously or asynchronously biaxially stretched, heat-set, and then cooled.

[0025] In a preferred embodiment of the present invention, the mixing conditions under the pressure conditions include: a pressure of 0.2-10MPa, preferably a pressure of 0.2-3MPa; and / or a time of 10-150h, preferably 30-150h. According to the present invention, there are multiple options for mixing. Preferably, non-stirring mixing is used for mixing. It is further preferred that the container drives the material to rotate for mixing. It is further preferred that a low-speed drum is used as a mixing means. For the rotation speed, the selection range is relatively wide, and the preferred rotation speed is 10-200rpm.

[0026] According to the present invention, the range of selection of the standing conditions is relatively wide. In a preferred embodiment of the present invention, the standing conditions include: a time of 10-20 hours, and / or a temperature of 40-80°C.

[0027] According to the present invention, the preforming has a wide range of selection conditions for preforming. In a preferred embodiment of the present invention, the preforming has a preforming pressure of 5-50 MPa and a holding time of 10 s-10 min.

[0028] According to the present invention, the range of selection of the push extrusion conditions is relatively wide. In a preferred embodiment of the present invention, the compression ratio of the push extrusion is 10-200, preferably 10-30.

[0029] According to the present invention, the calendering conditions have a wide selection range. In a preferred embodiment of the present invention, the calendering pressure is 0.1-10 MPa, preferably 0.5-5 MPa.

[0030] According to the present invention, the stretching conditions have a wide selection range. In a preferred embodiment of the present invention, biaxial stretching is performed by simultaneously performing longitudinal stretching and transverse stretching. Preferably, the stretching temperature is 20-300°C, preferably 150-250°C.

[0031] According to the present invention, the range of conditions for selection is relatively wide. In a preferred embodiment of the present invention, the biaxial stretching is performed in a manner where the longitudinal stretching and the transverse stretching are performed asynchronously; preferably, the stretching temperature is 20-300°C, preferably 150-250°C.

[0032] According to the present invention, the heat setting conditions have a wide selection range. In a preferred embodiment of the present invention, the heat setting temperature is 300-380° C., and the heat setting time is 20 seconds to 300 seconds.

[0033] According to the present invention, the cooling conditions have a wide selection range. In a preferred embodiment of the present invention, the cooling rate is 5-100° C. / min.

[0034] In a more preferred embodiment of the present invention, the preparation method of the polytetrafluoroethylene porous membrane comprises mixing the raw materials of the polytetrafluoroethylene composite under pressure, preforming, pushing and extruding, calendering, synchronous / asynchronous biaxial stretching, heat setting, and cooling; preparing the polytetrafluoroethylene porous membrane; mixing under the pressure condition is a pressure condition of 0.2-10MPa, a standing time of 10-20h, and a temperature of 40-80°C, mixing the components in the polytetrafluoroethylene composite and preforming to a preforming pressure of 5-50MPa, and holding the pressure The time is 10s-10min; the compression ratio of the push extrusion is 10-200; the calendering is a calendering pressure of 0.1-10MPa; the synchronous biaxial stretching is that the longitudinal stretching and the transverse stretching are carried out simultaneously, and the stretching temperature is 20-300℃; the asynchronous biaxial stretching is that the longitudinal stretching and the transverse stretching are carried out sequentially, and the stretching temperature is 20-300℃; the heat setting temperature is 300-380℃, and the heat setting time is 20 seconds-300 seconds; the cooling is a cooling rate of 5-100℃ per minute until reaching room temperature.

[0035] The fifth object of the present invention is to provide an application of the polytetrafluoroethylene composite porous membrane described above in industrial filtration and medical protection materials.

[0036] Compared with the prior art, the advantages of the present invention are:

[0037] (1) A plurality of polytetrafluoroethylene resins of preferably two relatively standard densities are mixed and used, so that the product has composite characteristics and has the advantages of high barrier efficiency and good air permeability. The inventors of the present invention believe that the above advantages are due to the fact that the present invention combines the different tensile properties of different raw materials under the same conditions and their different microstructures. In the same stretching process, the two components of polytetrafluoroethylene show differentiated tensile properties and form different fiber structures, and the obtained porous membrane has a composite structure.

[0038] (2) The present invention adopts a specific composite extrusion aid and two polytetrafluoroethylene raw materials with different densities. The composite extrusion aid promotes the compatibility of two different polytetrafluoroethylene resins, thereby obtaining a composite material with the above advantages, taking into account both economy and functionality;

[0039] (3) The present invention adopts a specific method to mix the raw materials under pressure conditions, thereby obtaining a composite material with the above advantages. This may be because mixing under pressure conditions improves and accelerates the miscibility of the extrusion aid and the polytetrafluoroethylene resin, so that the prepared material has composite properties.

[0040] (4) The salt medium filtration efficiency of the composite material obtained by the method of the present invention is as high as 97%, and the air permeability rate is about 3L / min, which has the advantages of high barrier efficiency and good air permeability. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is a scanning electron microscope photograph of the polytetrafluoroethylene porous membrane prepared in Example 8;

[0042] Figure 2 This is a scanning electron microscope photograph of the polytetrafluoroethylene porous membrane prepared in Example 6;

[0043] Figure 3 This is a scanning electron microscope photo of the polytetrafluoroethylene porous membrane prepared in Comparative Example 1. Figure 1 , 2 And 3, it can be seen that Figure 1 and 2 contains two fibers with large differences in diameter, and Figure 3 There is only one fiber diameter in the film. It is confirmed that in the same stretching process, the two components of polytetrafluoroethylene show differentiated stretching properties, forming different fiber structures, and the obtained porous membrane has a composite structure. DETAILED DESCRIPTION

[0044] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0045] (1) Experimental basic equipment: The stretching equipment is a German Bruckner biaxial stretching machine.

[0046] (2) Instruments used for experimental data measurement: The relative standard density in the experiment was carried out in accordance with GB / T 1033.1. Electron microscope photos were taken by Hitachi S4800-SEM, COXEM EM-30AX + Shooting.

[0047] In the following examples, the sources of some raw materials of the present invention are described in the examples, and other raw materials, unless otherwise specified, are conventional commercially available products.

[0048] Example 1

[0049] 1 kg of polytetrafluoroethylene resin (Shandong Dongyue DF205, average relative standard density 2.165), 1 kg of polytetrafluoroethylene resin (DuPont 605xt, average relative standard density 2.16), 0.1 kg of aviation kerosene (3#), and 0.1 kg of isoparaffin (ExxonMobil Isopar G) were mixed at 0.5 MPa for 30 hours (the sealed tank was rotated at 50 rpm for 30 hours to fully mix the resin powder and the extrusion aid), and allowed to stand at 40°C for 10 hours to obtain a polytetrafluoroethylene composite.

[0050] Example 2

[0051] 1 kg of polytetrafluoroethylene resin (Shanghai San Ai Fu FR203A-2, average relative standard density 2.18), 2 kg of polytetrafluoroethylene resin (Japan Daikin F106, average relative standard density 2.158), 0.4 kg of aviation kerosene (5#), and 0.1 kg of isoparaffin (ExxonMobil Isopar M) were mixed at 0.2 MPa for 120 h (the sealed tank was rotated at 50 rpm for 120 h to fully mix the resin powder and the extrusion aid), and allowed to stand at 80°C for 20 h to obtain a polytetrafluoroethylene composite.

[0052] Example 3

[0053] 3 kg of polytetrafluoroethylene resin (Shandong Dongyue DF205, average relative standard density 2.165), 1 kg of polytetrafluoroethylene resin (Sichuan Chenguang CGF216Y, average relative standard density 2.15), 0.8 kg of white oil (3#), and 1.2 kg of aviation kerosene (3#) were mixed at 2 MPa for 100 h (the sealed can was rotated at 50 rpm for 100 h to allow the resin powder and the extrusion aid to be fully mixed), and allowed to stand at 60°C for 15 h to obtain a polytetrafluoroethylene composite.

[0054] Example 4

[0055] 1 kg of polytetrafluoroethylene resin (Sichuan Chenguang CGF216G, average relative standard density 2.162), 4 kg of polytetrafluoroethylene resin (DuPont 605xt, average relative standard density 2.16), 0.1 kg of aviation kerosene (3#), and 0.1 kg of isoparaffin (ExxonMobil Isopar G) were mixed at 0.5 MPa for 150 hours (the sealed tank was rotated at 50 rpm for 150 hours to fully mix the resin powder and the extrusion aid), and allowed to stand at 80°C for 10 hours to obtain a polytetrafluoroethylene composite.

[0056] Example 5

[0057] 1 kg of polytetrafluoroethylene resin (Sichuan Chenguang CGF216G, average relative standard density 2.162), 1 kg of polytetrafluoroethylene resin (Sichuan Chenguang CGF216Y, average relative standard density 2.15), 0.1 kg of naphtha, and 0.4 kg of isoparaffin (ExxonMobil Isopar G) were mixed at 0.5 MPa for 50 hours (the sealed tank was rotated at 50 rpm for 50 hours to allow the resin powder and the extrusion aid to be fully mixed), and allowed to stand at 40°C for 20 hours to obtain a polytetrafluoroethylene composite.

[0058] Example 6

[0059] The polytetrafluoroethylene composite in Example 4 was subjected to preforming (pressure of 10 MPa, holding time of 1 min), push extrusion (compression ratio of 20), calendering (pressure of 5 MPa), simultaneous biaxial stretching (stretching temperature of 150°C), heat setting (temperature of 300°C, duration of 60 seconds), and cooling (cooling rate of 30°C per minute) to prepare a polytetrafluoroethylene porous membrane.

[0060] Example 7

[0061] The polytetrafluoroethylene composite in Example 5 was subjected to preforming (pressure of 5 MPa, holding time of 30 s), push extrusion (compression ratio of 25), calendering (pressure of 3 MPa), asynchronous biaxial stretching (longitudinal stretching temperature of 200 degrees, transverse stretching temperature of 70°C), heat setting (temperature of 340°C, duration of 30 seconds), and cooling (cooling rate of 30°C per minute) to prepare a polytetrafluoroethylene porous membrane.

[0062] Example 8

[0063] The polytetrafluoroethylene composite in Example 1 was subjected to preforming (pressure of 30 MPa, holding time of 3 min), push extrusion (compression ratio of 50), calendering (pressure of 10 MPa), simultaneous biaxial stretching (stretching temperature of 250°C), heat setting (temperature of 380°C, duration of 20 seconds), and cooling (cooling rate of 50°C per minute) to prepare a polytetrafluoroethylene porous membrane.

[0064] Example 9

[0065] The polytetrafluoroethylene composite in Example 2 was subjected to preforming (pressure of 50 MPa, holding time of 10 s), push extrusion (compression ratio of 10), calendering (pressure of 0.5 MPa), asynchronous biaxial stretching (longitudinal stretching temperature of 250 degrees, transverse stretching temperature of 150°C), heat setting (temperature of 300°C, duration of 300 seconds), and cooling (cooling rate of 15°C per minute) to prepare a polytetrafluoroethylene porous membrane.

[0066] Example 10

[0067] The polytetrafluoroethylene composite in Example 3 was subjected to preforming (pressure of 15 MPa, holding time of 30 s), push extrusion (compression ratio of 15), calendering (pressure of 2 MPa), asynchronous biaxial stretching (longitudinal stretching temperature of 300 degrees, transverse stretching temperature of 200°C), heat setting (temperature of 320°C, duration of 100 seconds), and cooling (cooling rate of 40°C per minute) to prepare a polytetrafluoroethylene porous membrane.

[0068] Comparative Example 1

[0069] 2kg of polytetrafluoroethylene resin (DuPont 605xt, average relative standard density of 2.16) and 0.2kg of aviation kerosene were mixed at normal pressure for 50 hours and allowed to stand at 60°C for 15 hours to obtain a polytetrafluoroethylene composite. The polytetrafluoroethylene porous membrane was prepared through preforming (pressure of 10MPa, holding time of 1min), push extrusion (compression ratio of 20), calendering (pressure of 5MPa), synchronous biaxial stretching (stretching temperature of 150°C), heat setting (temperature of 300°C, duration of 60 seconds), and cooling (cooling rate of 30°C per minute).

[0070] Comparative Example 2

[0071] 2kg of polytetrafluoroethylene resin (Shandong Dongyue DF205, average relative standard density 2.165) and 0.6kg of isoparaffin (ExxonMobil Isopar G) were mixed at normal pressure for 80 hours and allowed to stand at 80°C for 10 hours to obtain a polytetrafluoroethylene composite. The polytetrafluoroethylene porous membrane was prepared through preforming (pressure of 10MPa, holding time of 1min), push extrusion (compression ratio of 20), calendering (pressure of 5MPa), asynchronous biaxial stretching (longitudinal stretching temperature of 300°C, transverse stretching temperature of 150°C), heat setting (temperature of 300°C, duration of 60 seconds), and cooling (cooling rate of 30°C per minute).

[0072] Comparative Example 3

[0073] The polytetrafluoroethylene composite was prepared according to the method of Example 1, except that the mixture was mixed at normal pressure for 30 hours and allowed to stand at 40° C. for 10 hours to obtain the polytetrafluoroethylene composite. Then, a polytetrafluoroethylene porous membrane was prepared according to Example 8.

[0074] Test example

[0075] The porous membranes prepared in Examples 6-10 and Comparative Examples 1-2 were tested for salt medium filtration efficiency using the national standard GB / T 32610-2016 Appendix A method, with the test medium being NaCl particles and the test flow rate being 85 L / min. The porous membranes prepared were tested for air permeability using the national standard GB / T5453-1997 method, with the test pressure being 7 kPa and the test area being 20 cm 2 The above test results are shown in Table 1.

[0076] Table 1

[0077]

[0078]

[0079] As can be seen from Table 1, the salt medium filtration efficiency of the polytetrafluoroethylene composite porous membrane in the embodiment of the present invention is not less than 95%; at a pressure of 7 kPa and a test area of ​​20 cm 2 The air permeability under the conditions is greater than 2.2 L / min. It can be seen that the porous membrane obtained by using the raw materials of the present invention has fibers of different thicknesses, forming different fiber structures, and the obtained porous membrane has a composite structure, which can take into account both air permeability and barrier effect.

Claims

1. A polytetrafluoroethylene compound, comprising component A, component B and component C; The components A and B are both polytetrafluoroethylene resins, the average relative standard density of the component A is greater than the average relative standard density of the component B; and the component C is an extrusion aid; The preparation method of the polytetrafluoroethylene compound comprises mixing the components including the component A, the component B and the component C; the mixing is performed under pressure, and the mixing pressure is 0.2-10 MPa.

2. The polytetrafluoroethylene composite according to claim 1, characterized in that: The average relative standard density of component A and component B is 2.1-2.2 g / cm 3 between.

3. The polytetrafluoroethylene composite according to claim 1, characterized in that: The average relative standard density of component A is 2.161-2.2 g / cm 3 and / or, The average relative standard density of component B is 2.13-2.160 g / cm 3 and / or, The thermal instability coefficients of component A and component B are each no greater than 50.

4. The polytetrafluoroethylene composite according to any one of claims 1 to 3, characterized in that: In terms of weight percentage, relative to the total weight of the polytetrafluoroethylene composite, the content of component A is 5-90 weight %, the content of component B is 5-90 weight %, and the content of component C is 5-50 weight %.

5. The polytetrafluoroethylene composite according to any one of claims 1 to 3, characterized in that: In terms of weight percentage, relative to the total weight of the polytetrafluoroethylene composite, the content of component A is 10-50 weight %, the content of component B is 30-70 weight %, and the content of component C is 5-30 weight %.

6. The polytetrafluoroethylene composite according to any one of claims 1 to 3, characterized in that: The component A and the component B are each independently selected from polytetrafluoroethylene resin obtained by dispersion polymerization; and / or, The component C is selected from at least two of aviation kerosene, white oil, naphtha, isoparaffin and kerosene.

7. The polytetrafluoroethylene composite according to claim 6, characterized in that: The component C is selected from at least two of aviation kerosene, white oil and isoparaffin.

8. The polytetrafluoroethylene composite according to claim 7, characterized in that: The component C is selected from aviation kerosene and isoparaffins.

9. The polytetrafluoroethylene composite according to claim 8, characterized in that: Based on the total weight of the component C being 100%, the content of the aviation kerosene is 10-50% by weight, and the content of the isoparaffin is 50-90% by weight.

10. A method for preparing the polytetrafluoroethylene compound according to any one of claims 1 to 9, comprising mixing the components including the component A, the component B and the component C, wherein the mixing is performed under pressure, and the mixing pressure is 0.2-10 MPa.

11. The preparation method according to claim 10, characterized in that: The mixing time is 10-150h.

12. The preparation method according to claim 11, characterized in that: The mixing method is non-stirring mixing.

13. The preparation method according to claim 12, characterized in that: The mixing method is to rotate the container to drive the materials in the container to mix.

14. The preparation method according to claim 13, characterized in that: The mixing method is to rotate the container to drive the materials in the container to mix, and the rotation speed is 10-200 rpm.

15. The preparation method according to claim 10, characterized in that The mixing includes standing.

16. The preparation method according to claim 15, characterized in that: The standing time is 10-20 hours; and / or the standing temperature is 40-80°C.

17. A polytetrafluoroethylene composite porous membrane, wherein the polytetrafluoroethylene composite porous membrane is made of the polytetrafluoroethylene compound according to any one of claims 1 to 9.

18. The polytetrafluoroethylene composite porous membrane according to claim 17, characterized in that: The salt medium filtration efficiency of the polytetrafluoroethylene composite porous membrane is not less than 95%; and / or, The polytetrafluoroethylene composite porous membrane is tested at a pressure of 7 kPa and a test area of ​​20 cm 2 The air permeability under the conditions is 2-10L / min.

19. The polytetrafluoroethylene composite porous membrane according to claim 18, characterized in that: The polytetrafluoroethylene composite porous membrane is tested at a pressure of 7 kPa and a test area of ​​20 cm 2 The air permeability under the conditions is 2-5 L / min.

20. A method for preparing the polytetrafluoroethylene composite porous membrane according to any one of claims 17 to 19, comprising forming a membrane from the polytetrafluoroethylene composite.

21. The preparation method according to claim 20, characterized in that: The method comprises the steps of preforming, pushing and extruding, calendering, biaxial stretching, heat setting and cooling the polytetrafluoroethylene compound.

22. The preparation method according to claim 21, characterized in that: The preforming pressure is 5-50 MPa, and the holding time is 10 s-10 min; and / or, The compression ratio of the push extrusion is 10-200; and / or, The calendering pressure is 0.1-10 MPa.

23. The preparation method according to claim 21, characterized in that: The biaxial stretching is performed in a manner where longitudinal stretching and transverse stretching are performed simultaneously.

24. The preparation method according to claim 21, characterized in that: The biaxial stretching is carried out in a manner of simultaneously carrying out longitudinal stretching and transverse stretching; the stretching temperature is 20-300°C.

25. The preparation method according to claim 21, characterized in that: The biaxial stretching is performed in a manner that the longitudinal stretching and the transverse stretching are performed asynchronously.

26. The preparation method according to claim 21, characterized in that: The biaxial stretching is performed in a manner that longitudinal stretching and transverse stretching are performed asynchronously, and the stretching temperature is 20-300°C.

27. The preparation method according to claim 21, characterized in that: The heat setting temperature is 300-380°C and the heat setting time is 20-300 seconds; and / or, The cooling rate of the cooling is 5-100°C / min.

28. Use of the polytetrafluoroethylene composite porous membrane according to any one of claims 17 to 19 in industrial filtration and medical protection materials.