A manganese-loaded silver-loaded catalytic adsorbent for flue gas demercuration and denitrification, and its preparation method and application
By first loading manganese oxide on EVS-10 molecular sieve, and then loading silver nanoparticles on the manganese-loaded silver catalytic adsorbent, the problem of synergistic removal of elemental mercury and nitrogen oxides in flue gas is solved and efficient removal effect is achieved. And reduces the cost, suitable for industrial applications.
Patent Information
- Application Number
- CN202111273160.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Existing flue gas treatment technology is difficult to effectively remove elemental mercury (Hg0) and nitrogen oxides (NOx) in flue gas, and existing catalysts cannot achieve synergistic removal effects.
Using a manganese-loaded silver catalytic adsorbent, the EVS-10 molecular sieve is first loaded with manganese oxide and then silver nanoparticles to achieve synergistic removal of Hg0 and NOx in flue gas. The catalytic adsorbent includes carrier EVS-10 molecular sieve, manganese oxide and silver nanoparticles. A specific preparation method ensures high dispersion of manganese ions and controllable size of silver nanoparticles.
It achieves efficient and coordinated removal of Hg0 and NOx in coal-fired flue gas, reduces overall costs, is suitable for industrial production and equipment upgrading, and has good adaptability and compatibility.
Smart Images

Figure BDA0003329329670000101 
Figure BDA0003329329670000111
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of environmental protection and air pollution control, and in particular to a manganese- and silver-loaded catalytic adsorbent for flue gas demercurization and denitrification, and a preparation method and application thereof. Background Art
[0002] The key to removing mercury from flue gas of coal-fired power plants is to control Hg 0 Coal-fired power plants are considered to be one of the most important sources of anthropogenic mercury emissions. Mercury is a toxic heavy metal that poses serious harm to human health and the ecological environment. Mercury in flue gas mainly includes the following three forms: Hg 2+ , Hg p and Hg 0 Based on the existing treatment methods, Hg in flue gas p Since it combines with fly ash, it can be removed by particulate matter control equipment such as bag filters or electrostatic precipitators; Hg in flue gas 2+ It is soluble in water and can therefore be removed efficiently by the pollutant control equipment wet flue gas desulfurization device; 0 Due to its insolubility in water, volatility and low-temperature stability, existing treatment methods and equipment are unable to effectively remove elemental mercury from flue gas, which will cause elemental mercury to be emitted into the atmosphere.
[0003] The two most widely studied methods of mercury removal are adsorbent demercuration and catalytic oxidation demercuration. 0 Through physical or chemical adsorption to the adsorbent surface, and then removed by the particulate matter control equipment; catalytic oxidation demercuration is to remove Hg 0 Highly efficient oxidation to Hg 2+ , and then removed by the wet desulfurization device. EVS-10 is a type of molecular sieve in which vanadium completely replaces the titanium in the titanium silicate molecular sieve ETS-10. It also carries silver nanoparticles and vanadium active components, and has a certain ability to adsorb and catalyze the oxidation of Hg 0 However, it has a single function and can only be used to control a single pollutant, mercury, but does not have the ability to remove nitrogen oxides.
[0004] In addition to elemental mercury, nitrogen oxides are also a common air pollutant produced by coal combustion. Nitrogen oxides can cause acid rain and greenhouse effect. The proportion of NO in nitrogen oxides (NOx) is more than 95%, so the key to removing nitrogen oxides is to remove NO. At present, the most effective and widely used technology for removing NO from coal-fired flue gas is NH3 selective catalytic reduction (SCR) technology. The SCR catalysts currently studied are mainly prepared by loading metal oxides such as V2O5, CuO, Cr2O3, CeO2, Fe2O3, MnO2, Co2O3 on carriers such as Al2O3, SiO2, TiO2, ZrO2, carbon materials and molecular sieves. However, the existing catalytic adsorbents still cannot achieve the effect of synergistic demercuration and denitrification. Summary of the invention
[0005] The purpose of the present disclosure is to provide a manganese- and silver-loaded catalytic adsorbent for flue gas demercuration and denitrification, and a preparation method and application thereof, wherein the catalytic adsorbent can achieve synergistic removal of mercury and nitrogen oxides.
[0006] In order to achieve the above-mentioned objectives, the first aspect of the present disclosure provides a manganese-loaded silver-loaded catalytic adsorbent for flue gas demercurization and denitrification, the catalytic adsorbent comprising a carrier and an active component and silver nanoparticles loaded on the carrier; wherein the carrier comprises EVS-10 molecular sieve, and the active component comprises manganese oxide.
[0007] Optionally, based on the total weight of the catalytic adsorbent, the mass fraction of the carrier is 45-98 weight %, the mass fraction of the silver nanoparticles is 1-40 weight %, and the mass fraction of the active component is 1-15 weight %.
[0008] The second aspect of the present disclosure provides a method for preparing the catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure, comprising the following steps:
[0009] (1) mixing EVS-10 molecular sieve, a manganese source and water to obtain a first mixture;
[0010] (2) mixing the first mixture and the alkaline solution, adding an oxidant to contact the manganese source for oxidation reaction to obtain a first solid product loaded with manganese oxide;
[0011] (3) mixing the first solid product, a silver source and water to perform ion exchange between the silver source and the EVS-10 molecular sieve in the first solid product, and then washing and drying to obtain a second solid product;
[0012] (4) calcining the second solid product to obtain the catalytic adsorbent.
[0013] Optionally, in step (1), the weight ratio of the EVS-10 molecular sieve, the manganese source and water is (0.225-0.2375): (0.018-0.07): 1;
[0014] Optionally, the manganese source is a soluble manganese salt, and the soluble manganese salt is selected from one or more of manganese acetate, manganese chloride and manganese nitrate.
[0015] Optionally, the first mixture further comprises a dispersing aid; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, preferably polymethacrylic acid; preferably, the weight ratio of the dispersing aid to the manganese source is (2-6): (0.72-2.8);
[0016] Optionally, step (1) comprises: mixing the manganese source, water and the optional dispersing aid, performing ultrasonic treatment and adding the EVS-10 molecular sieve to obtain the first mixture.
[0017] Optionally, in step (2), the alkaline solution includes sodium hydroxide solution; the oxidant includes hydrogen peroxide; further preferably, the concentration of the hydrogen peroxide is 25 to 35 weight %; preferably, the volume ratio of the hydrogen peroxide to the first mixture is (0.075 to 0.125):1.
[0018] Optionally, the conditions of the oxidation reaction in step (2) include: a reaction temperature of 40 to 80° C. and a reaction time of 0.5 to 2 h;
[0019] Optionally, step (2) includes: mixing the alkaline solution and the first solid product, ultrasonically treating the mixture for 5 to 30 minutes, and then adding the oxidant to carry out the oxidation reaction; and filtering, washing, drying, and then sieving the oxidation reaction product to obtain the first solid product; wherein the drying temperature of the oxidation reaction product is 70 to 110°C.
[0020] Optionally, in step (3), the silver source includes silver nitrate; preferably, the silver nitrate is first reacted with water to form a silver nitrate solution, and then the first solid product is added to the silver nitrate solution to carry out the oxidation reaction;
[0021] Preferably, the weight ratio of silver nitrate to the EVS-10 molecular sieve is (4.25-6): (9-9.5);
[0022] Optionally, after the mixing in step (3), the mixture further comprises: magnetic stirring in a light-proof environment for 1 to 24 hours; and optionally, the drying temperature in step (3) is 80 to 110° C.
[0023] Optionally, in step (4), the calcination treatment conditions include: in an inert atmosphere, a calcination temperature of 150 to 400° C., and a calcination time of 0.5 to 2 hours; wherein the inert atmosphere is nitrogen or argon.
[0024] The third aspect of the present disclosure provides application of the catalytic adsorbent described in the first aspect of the present disclosure in the field of flue gas demercurization and denitrification; optionally, the flue gas is flue gas from a coal-fired power plant.
[0025] Through the above technical scheme, the present invention provides a manganese-loaded silver-loaded catalytic adsorbent for flue gas demercuration and denitrification, and its preparation method and application. The present invention loads active components including manganese oxide and silver nanoparticles on EVS-10 molecular sieve in the order of "first loading active components, then loading silver nanoparticles". The obtained manganese-loaded silver-loaded catalytic adsorbent can both adsorb and catalytically oxidize Hg 0 , and can also catalytically reduce NOx, achieving the reduction of Hg in coal-fired flue gas 0 and NOx synergistic removal effect. In the preparation process of the catalytic adsorbent, the manganese ions have high dispersion and avoid agglomeration, and the manganese oxide loaded on the catalytic adsorbent finally obtained also has high dispersion; the size of the silver nanoparticles is easy to control by adjusting the process parameters, and the size controllability of the silver nanoparticles is achieved. The catalytic adsorbent provided by the present invention is relatively simple to synthesize in terms of process, can avoid agglomeration during repeated recycling, can be recycled, greatly reduces the overall cost, and is suitable for industrial production; the process has good adaptability and compatibility, is suitable for use in series with dust removal and desulfurization equipment, and is particularly suitable for enterprises with desulfurization and dust removal equipment to expand their use for mercury removal upgrades, reduces equipment installation and use costs, and has industrial application prospects.
[0026] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0027] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0028] The inventors of the present disclosure surprisingly found in a large number of experiments that when EVS-10 molecular sieve is used as a carrier, the active components containing manganese oxide are first loaded and then silver nanoparticles are loaded, the resulting catalytic adsorbent can not only synergistically remove elemental mercury and nitrogen oxides in coal-fired flue gas, but also the mercury removal rate and denitrification efficiency can reach a relatively high level.
[0029] A first aspect of the present disclosure provides a manganese- and silver-loaded catalytic adsorbent for flue gas demercuration and denitrification, the catalytic adsorbent comprising a carrier and an active component and silver nanoparticles loaded on the carrier; wherein the carrier comprises an EVS-10 molecular sieve, and the active component comprises manganese oxide; wherein the active component is first loaded on the EVS-10 molecular sieve, and the silver nanoparticles are subsequently loaded on the EVS-10 molecular sieve.
[0030] The present invention loads active components including manganese oxide and silver nanoparticles on EVS-10 molecular sieve in the order of "loading active components first and then loading silver nanoparticles", and the obtained manganese-loaded and silver-loaded catalytic adsorbent can both adsorb and catalytically oxidize Hg 0 , and can also catalytically reduce NOx, achieving the reduction of Hg in coal-fired flue gas 0 The catalytic adsorbent has a synergistic removal effect on NOx. In the preparation process of the catalytic adsorbent, the manganese ions have a high dispersion and avoid agglomeration, and the manganese oxide loaded on the catalytic adsorbent finally obtained also has a high dispersion; the size of the silver nanoparticles is easy to control by adjusting the process parameters (temperature, roasting atmosphere, etc.), and the size controllability of the silver nanoparticles is achieved. The catalytic adsorbent provided by the present disclosure is relatively simple to synthesize in terms of process, can avoid agglomeration during repeated recycling, can be recycled, greatly reduces the overall cost, and is suitable for industrial production.
[0031] In the present disclosure, the manganese oxide is a type of manganese oxide known to those skilled in the art that can be used as a catalyst active component.
[0032] In the present disclosure, the EVS-10 molecular sieve is used as a carrier and loaded with manganese oxide and silver nanoparticles, wherein the silver nanoparticles can efficiently adsorb elemental mercury, the vanadium active component in the EVS-10 molecular sieve framework can also catalytically oxidize part of the elemental mercury, and the manganese oxide has good denitrification performance and the ability to catalytically oxidize elemental mercury, and can synergistically remove elemental mercury and nitrogen oxides in coal-fired flue gas, so that the catalytic adsorbent has excellent mercury removal efficiency and high denitrification efficiency, and can also achieve elemental mercury (Hg 0 ) for efficient removal.
[0033] In one embodiment, based on the total weight of the catalytic adsorbent, the mass fraction of the carrier is 45-98 weight percent, the mass fraction of the silver nanoparticles is 1-40 weight percent, and the mass fraction of the active component is 1-15 weight percent. When the content of each component in the catalytic adsorbent provided by the present disclosure is within the range of this embodiment, the obtained catalytic adsorbent can achieve a good synergistic removal effect of elemental mercury and nitrogen oxides.
[0034] In a specific embodiment, the carrier is an EVS-10 molecular sieve; in terms of element molar amount, the molar ratio of Si:Na:K:V in the EVS-10 molecular sieve is 3.92:1.39:0.48:1. In the present disclosure, the chemical composition of the EVS-10 molecular sieve is determined by XRF spectroscopy.
[0035] The second aspect of the present disclosure provides a method for preparing a catalytic adsorbent for mercury removal and denitrification, comprising the following steps:
[0036] (1) mixing EVS-10 molecular sieve, a manganese source and water to obtain a first mixture;
[0037] (2) mixing the first mixture and the alkaline solution, adding an oxidant to contact the manganese source for oxidation reaction to obtain a first solid product loaded with manganese oxide;
[0038] (3) mixing the first solid product, a silver source and water to perform ion exchange between the silver source and the EVS-10 molecular sieve in the first solid product, and then washing and drying to obtain a second solid product;
[0039] (4) calcining the second solid product to obtain the catalytic adsorbent.
[0040] In the preparation method provided by the present disclosure, a manganese source and an EVS-10 molecular sieve are first dispersed in water, and after the manganese ions in the first mixture are mixed with an alkaline solution, a dispersed system can be obtained, and then an oxidant, such as hydrogen peroxide, is added to the dispersed system. The hydrogen peroxide contacts with the manganese ions in the system and undergoes an oxidation reaction, forming a monodisperse or very small (nanometer-sized) manganese oxide on the surface of the molecular sieve as an active component, and separating to obtain a first solid product; then the first solid product is mixed with a silver source solution, and the silver ions react with the Na in the molecular sieve. + and K + Ion exchange is performed, and then silver nanoparticles are formed on the EVS-10 molecular sieve by calcination. During the calcination process, the size of the silver nanoparticles can be controlled by temperature and calcination atmosphere. The synthesis method provided by the present disclosure is stable and reliable, the comprehensive use cost of the catalytic adsorbent is low, and it has good industrial application prospects.
[0041] EVS-10 molecular sieve can be prepared by existing methods or purchased commercially. For example, EVS-10 molecular sieve can be prepared according to existing methods, for example, according to the method disclosed in the document Zijian Zhou, Tiantian Cao, et al. "Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elementalmercury removal from flue gas". Journal of Hazardous Materials, 375 (2019) 1-8. In a specific embodiment, the EVS-10 molecular sieve used in the present disclosure can be prepared by a hydrothermal method, specifically comprising: dissolving sodium silicate in deionized water; then adding NaOH, KCl, NaF and NaCl to the solution to obtain solution A. Then VOSO4 is dissolved in deionized water to obtain solution B. Solution A and solution B are mixed and stirred, and aged at room temperature. The aged mixture is transferred to an autoclave for further aging. The synthesized product is washed with deionized water and dried to obtain an EVS-10 molecular sieve. During the preparation process, the amount of each reactant and the reaction conditions can be adjusted according to actual needs.
[0042] In one embodiment, in step (1), the weight ratio of the EVS-10 molecular sieve, the manganese source and water is (0.225-0.2375): (0.018-0.07): 1.
[0043] In one embodiment, the manganese source is a soluble manganese salt, and the soluble manganese salt is selected from one or more of manganese acetate, manganese chloride and manganese nitrate.
[0044] In a preferred embodiment, the first mixture further includes a dispersing aid; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, preferably polymethacrylic acid; preferably, the weight ratio of the dispersing aid to the manganese source is (2-6): (0.72-2.8). In a further embodiment, step (1) further includes: mixing the manganese source, water and the optional dispersing aid, performing ultrasonic treatment and adding the EVS-10 molecular sieve to obtain the first mixture.
[0045] In the present disclosure, a dispersing aid can be used to form a complex with Mn ions in a solution so that the Mn ions are uniformly dispersed in the system in the form of a complex, thereby improving the demercuration and denitrification efficiency of the prepared catalytic adsorbent. In the present disclosure, a manganese source and a dispersing aid are simultaneously introduced in the process of preparing the catalytic adsorbent, and the Mn ions form a complex (chelate) with the dispersing aid, so that it will not precipitate when an alkaline solution (such as sodium hydroxide) is subsequently added, and the uniformly dispersed Mn ion complex (for example) can be stably present in the system; after the addition of an oxidant (such as hydrogen peroxide), the manganese ions in the system are oxidized on the surface of the EVS-10 molecular sieve into a monodisperse or very small (nano-sized) manganese oxide active component, which has a high degree of dispersion and is conducive to improving the catalytic adsorption performance.
[0046] In one embodiment, in step (2), the alkaline solution includes sodium hydroxide solution; the oxidant includes hydrogen peroxide; further preferably, the concentration of the hydrogen peroxide is 30 weight %; preferably, the volume ratio of the hydrogen peroxide to the first mixture is (0.075-0.125):1.
[0047] In one embodiment, the conditions of the oxidation reaction in step (2) include: a reaction temperature of 40 to 80° C. and a reaction time of 0.5 to 2 h.
[0048] In one embodiment, step (2) comprises: mixing the alkaline solution and the first solid product, ultrasonically treating the mixture for 5 to 30 minutes, and then adding the oxidant to carry out the oxidation reaction; filtering, washing, drying, and then sieving the oxidation reaction product, taking the sieve underflow to obtain the first solid product; wherein the oxidation reaction product is dried at a temperature of 70 to 110° C. For example, after drying and cooling to room temperature, the mixture is sieved using a 100-mesh sieve, and the sieve underflow is taken as the final catalytic adsorbent.
[0049] In one embodiment, in step (3), in step (3), the silver source includes silver nitrate; preferably, the silver nitrate is first reacted with water to form a silver nitrate solution, and then the first solid product is added to the silver nitrate solution to carry out the oxidation reaction;
[0050] Preferably, the weight ratio of silver nitrate to the EVS-10 molecular sieve is (4.25-6): (9-9.5);
[0051] Optionally, after the mixing in step (3), the mixture further comprises: magnetic stirring in a light-proof environment for 1 to 24 hours; and optionally, the drying temperature in step (3) is 80 to 110° C.
[0052] In the present disclosure, the "light-proof environment" refers to operations well known to those skilled in the art when it comes to silver nitrate solution, such as using a brown container or wrapping it with light-proof paper in a darker environment.
[0053] In one embodiment, in step (4), the calcination conditions include: calcination temperature of 150-400°C and calcination time of 0.5-2 hours under an inert atmosphere, wherein the inert atmosphere is nitrogen or argon. Specifically, the calcination device can be a tubular furnace.
[0054] The third aspect of the present disclosure provides application of the catalytic adsorbent described in the first aspect of the present disclosure in the field of flue gas demercurization and denitrification; optionally, the flue gas is flue gas from a coal-fired power plant.
[0055] The present invention is further described below in conjunction with specific embodiments, but the scope of protection claimed by the present invention is not limited to the scope described in the embodiments.
[0056] The chemicals used in each example can be obtained through public commercial channels.
[0057] The EVS-10 molecular sieve used in the following examples and comparative examples was prepared according to the method disclosed in Zijian Zhou, Tiantian Cao, et al. "Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elemental mercury removal from flue gas". Journal of Hazardous Materials, 375 (2019) 1-8.
[0058] The 30% hydrogen peroxide used below refers to a solution with a mass percentage of 30% hydrogen peroxide.
[0059] The ultrasonic treatment in the present disclosure uses a conventional ultrasonic device to make the materials mixed or dispersed more uniformly.
[0060] Example 1
[0061] (1) 2.8 g Mn(CH3COO)2·4H2O and 6.0 g PMAA were dissolved in 40 mL deionized water, and 9.0 g EVS-10 molecular sieves were added during ultrasonic treatment;
[0062] (2) slowly adding 25 mL of 2 mol / L sodium hydroxide solution, ultrasonically treating for 15 minutes, then adding 5 mL of 30 wt % hydrogen peroxide, reacting at 60° C. for 1 hour, filtering out the solid sample, repeatedly washing with ethanol and deionized water, then drying the sample at 80° C., sieving with a 100-mesh sieve, taking the particles under the sieve, and obtaining an EVS-10 molecular sieve loaded with active component manganese oxide;
[0063] (3) Weigh 4.3 g of AgNO3 and dissolve it in 100 ml of deionized water. Then add the molecular sieve loaded with the active component manganese oxide. Stir magnetically in a light-proof environment for 6 h. Then filter and rinse repeatedly with deionized water. Dry at 80° C. and then calcine in a tubular furnace at 250° C. in a nitrogen atmosphere for 1 hour to obtain a catalytic adsorbent loaded with manganese oxide and silver nanoparticles, which is recorded as sample Y1.
[0064] Comparative Example 1
[0065] The catalytic adsorbent was prepared by similar steps to Example 1, except that the EVS-10 molecular sieve was replaced with the commercially available ETS-10 molecular sieve. The other preparation steps were the same as those in Example 1, and a catalytic adsorbent loaded with manganese oxide and silver particles was obtained, which was recorded as sample D-1.
[0066] Example 2
[0067] (1) 0.72 g MnCl2 and 2.0 g PMAA were dissolved in 40 mL deionized water, and 9.5 g EVS-10 molecular sieves were added during ultrasonic treatment;
[0068] (2) slowly adding 12 mL of 2 mol / L sodium hydroxide solution, ultrasonically treating for 15 minutes, then adding 3 mL of 30 wt % hydrogen peroxide, reacting at 60° C. for 1 hour, filtering out the solid sample, repeatedly washing with ethanol and deionized water, then drying the sample at 80° C., and then sieving with a 100-mesh sieve, taking the particles under the sieve to obtain the EVS-10 molecular sieve loaded with the active component manganese oxide;
[0069] (3) Weigh 6 g of AgNO3 and dissolve it in 100 ml of deionized water, then add the above-mentioned molecular sieve loaded with active component manganese oxide, magnetically stir for 24 hours in a light-proof environment, then filter and repeatedly rinse with deionized water, dry at 100°C, and then place it in a tube furnace for calcination at 300°C in an argon atmosphere for 1 hour to obtain a catalytic adsorbent loaded with manganese oxide and silver nanoparticles, which is recorded as sample Y2.
[0070] Example 3
[0071] A preparation method similar to that of Example 1 was adopted, which differed from Example 1 in that no PMAA dispersing agent was added in step (1), and other raw materials and amounts, step operations and reaction conditions were the same as those in Example 1, to obtain a catalytic adsorbent loaded with manganese oxide and silver nanoparticles, which was recorded as sample Y3.
[0072] Comparative Example 2
[0073] Weigh 4.3 g of AgNO3 and dissolve it in 100 ml of deionized water, then add 10 g of EVS-10 molecular sieve, stir it magnetically in a dark environment for 6 h, then filter it, rinse it repeatedly with deionized water, dry it at 80 ° C, and then bake it in a tube furnace at 250 ° C in a nitrogen atmosphere for 1 hour. The catalytic adsorbent loaded with only silver nanoparticles is obtained, which is recorded as sample D-2.
[0074] The mass fractions of the carrier molecular sieve, manganese oxide and silver particles in the samples obtained from the above embodiments, comparative examples and comparative examples are listed in Table 1.
[0075] Table 1
[0076]
[0077]
[0078] The mass fraction of manganese oxide is expressed as MnO2.
[0079] Simulated smoke test example
[0080] The samples synthesized in the above examples and comparative examples were placed in a simulated flue gas experimental system to test the demercuration and denitrification performance. The simulated flue gas conditions are as follows: 5% O2, 12% CO2, 400ppm NO, 400ppm NH3, 600ppm SO2, 30ppm HCl, Hg 0 Concentration: 110 μg / m 3 , the balance gas is N2, the total flue gas flow rate is 500 mL / min, and the test temperature is 250°C. The experimental system for simulating flue gas can be any conventional experimental system in the art. The results of the mercury removal and denitrification tests are listed in Table 2 below.
[0081] Table 2
[0082] sample <![CDATA[Hg 0 Removal efficiency (%)]]> <![CDATA[NO x Removal efficiency (%)]]> Y1 100 95 D-1 87 77 Y2 100 92 Y3 100 74 D-2 100 21
[0083] According to Table 2 above, when Example 1 is compared with Comparative Example 1, the Hg content of the catalyst prepared by using EVS-10 molecular sieve in Example 1 is 0 Removal efficiency and NO x The removal efficiency is better.
[0084] Comparing Examples 1 to 3 of the present application with Comparative Example 2, the silver-loaded catalytic adsorbent prepared by the prior art in Comparative Example 2 can achieve a good removal efficiency of elemental mercury, but the removal efficiency of nitrogen oxides is extremely low, only 21%. The catalytic adsorbent samples prepared by the method provided by the present disclosure in Examples 1 to 3 can achieve simultaneous removal of Hg 0 and NO x .
[0085] Furthermore, by comparing Examples 1 to 2 with Example 3, it can be seen that the addition of a dispersing agent in Examples 1 to 2 results in a catalytic adsorbent having a higher Hg 0 Removal efficiency and NO x Removal efficiency.
[0086] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0087] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0088] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A manganese- and silver-loaded catalytic adsorbent for flue gas demercuration and denitrification, characterized in that: The catalytic adsorbent comprises a carrier and an active component and silver nanoparticles loaded on the carrier; wherein the carrier comprises an EVS-10 molecular sieve, and the active component comprises manganese oxide; wherein the active component is first loaded on the EVS-10 molecular sieve, and the silver nanoparticles are then loaded on the EVS-10 molecular sieve; The catalytic adsorbent is prepared by a method comprising the following steps: (1) mixing EVS-10 molecular sieve, a manganese source and water to obtain a first mixture; (2) after mixing the first mixture and the alkaline solution, adding an oxidant to contact the manganese source for oxidation reaction to obtain a first solid product loaded with manganese oxide; (3) mixing the first solid product, a silver source and water to perform ion exchange between the silver source and the EVS-10 molecular sieve in the first solid product, and then washing and drying to obtain a second solid product; (4) calcining the second solid product to obtain the catalytic adsorbent; The first mixture further comprises a dispersing aid; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride.
2. The catalytic adsorbent according to claim 1, characterized in that: Based on the total weight of the catalytic adsorbent, the mass fraction of the carrier is 45-98 weight %, the mass fraction of the silver nanoparticles is 1-40 weight %, and the mass fraction of the active component is 1-15 weight %.
3. The catalytic adsorbent according to claim 1, characterized in that: In step (1), the weight ratio of the EVS-10 molecular sieve, the manganese source and water is (0.225~0.2375):(0.018~0.07):
1.
4. The catalytic adsorbent according to claim 1, characterized in that: The manganese source is a soluble manganese salt, and the soluble manganese salt is selected from one or more of manganese acetate, manganese chloride and manganese nitrate.
5. The catalytic adsorbent according to claim 1, characterized in that: The dispersing aid is polymethacrylic acid.
6. The catalytic adsorbent according to claim 1, characterized in that: The weight ratio of the dispersing aid to the manganese source is (2-6): (0.72-2.8).
7. The catalytic adsorbent according to claim 1, characterized in that: Step (1) comprises: mixing the manganese source, water and the dispersing aid, performing ultrasonic treatment and adding the EVS-10 molecular sieve to obtain the first mixture.
8. The catalytic adsorbent according to claim 1, characterized in that: In step (2), the alkaline solution includes sodium hydroxide solution; and the oxidant includes hydrogen peroxide.
9. The catalytic adsorbent according to claim 8, characterized in that: The concentration of the hydrogen peroxide is 25-35% by weight.
10. The catalytic adsorbent according to claim 8, characterized in that: The volume ratio of the hydrogen peroxide solution to the first mixture is (0.075-0.125):
1.
11. The catalytic adsorbent according to claim 1, characterized in that: The conditions of the oxidation reaction in step (2) include: reaction temperature of 40-80° C., and reaction time of 0.5-2 h.
12. The catalytic adsorbent according to claim 11, characterized in that: Step (2) comprises: mixing the alkaline solution and the first solid product, subjecting the mixture to ultrasonic treatment for 5 to 30 minutes, and then adding the oxidant to carry out the oxidation reaction; and filtering, washing, drying, and then sieving the oxidation reaction product to obtain the first solid product; wherein the drying temperature of the oxidation reaction product is 70 to 110°C.
13. The catalytic adsorbent according to claim 1, characterized in that: In step (3), the silver source includes silver nitrate; the silver nitrate is first reacted with water to form a silver nitrate solution, and then the first solid product is added to the silver nitrate solution to carry out the oxidation reaction.
14. The catalytic adsorbent according to claim 13, characterized in that: The weight ratio of the silver nitrate to the EVS-10 molecular sieve is (4.25-6): (9-9.5).
15. The catalytic adsorbent according to claim 1, characterized in that: After the mixing in step (3), the method further comprises: magnetic stirring in a light-proof environment for 1 to 24 hours; the drying temperature in step (3) is 80 to 110°C.
16. The catalytic adsorbent according to claim 1, characterized in that: In step (4), the calcination treatment conditions include: in an inert atmosphere, a calcination temperature of 150-400° C., and a calcination time of 0.5-2 hours; wherein the inert atmosphere is nitrogen or argon.
17. Use of the manganese- and silver-loaded catalytic adsorbent according to any one of claims 1 to 16 in the field of flue gas mercury removal and denitrification.
18. The use according to claim 17, characterized in that The flue gas is flue gas from a coal-fired power plant.