Hydrogenation catalyst and its preparation method and application

By using a phosphorus-containing alumina carrier with specific infrared characteristics and controlling the proportion of hydrogenation active metal components, a hydrogenation catalyst with high activity and stability is prepared, which solves the problem of insufficient activity and stability of hydrogenation catalysts in the existing technology, and significantly Improved desulfurization and denitrification efficiency in wax oil hydrotreating.

CN116060048BActive Publication Date: 2024-10-11CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111270774.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-11
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Existing hydrogenation catalysts have insufficient activity stability and short service life in hydrocarbon oil hydrogenation reactions. Especially in the hydrotreating of wax oil fractions, the performance and activity cannot meet the requirements.

Method used

Using a phosphorus-containing alumina carrier with specific infrared characteristics, and controlling the carbon component content and hydrogenation active metal component ratio in the catalyst, the product is prepared through specific preparation methods, including precipitation, aging, roasting and impregnation processes. Highly active and stable hydrogenation catalyst.

Benefits of technology

Significantly improves the activity stability and service life of the hydrogenation catalyst, especially in wax oil hydrotreating, showing excellent desulfurization and denitrification activity, extending the service life of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003328673160000211
    Figure BDA0003328673160000211
  • Figure BDA0003328673160000212
    Figure BDA0003328673160000212
  • Figure BDA0003328673160000213
    Figure BDA0003328673160000213
Patent Text Reader

Abstract

The invention discloses a hydrogenation catalyst and a preparation method and application thereof. The hydrogenation catalyst comprises a carrier, a hydrogenation active metal component and a carbon component loaded on the carrier. Based on the total amount of the hydrogenation catalyst, the carbon component content in terms of element is 0.03-0.8% by weight, the carrier content is 40-85% by weight, and the hydrogenation active metal component satisfies the following relationship: 0.25≤n(VIB) / n(VIB+VIII)≤0.35, wherein n(VIB) represents the amount of substance of the VIB group metal element, and n(VIB+VIII) represents the sum of the amounts of substance of the VIB group metal element and the VIII group metal element; the carrier is phosphorus-containing aluminum oxide, and in the IR spectrum of the phosphorus-containing aluminum oxide, (I 3670 +I 3580 ) / (I 3770 +I 3720 ) is 1.9-2.8; among which, I 3670 3670cm ‑1 At the peak height, I 3580 3580cm ‑1 At the peak height, I 3770 3770cm ‑1 At the peak height, I 3720 3720cm ‑1 Compared with the prior art, the hydrogenation catalyst provided by the present invention adopts a specific carrier, and the catalyst contains a certain amount of carbon components, has better hydrodenitrogenation and hydrodesulfurization performance, and has a longer service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of hydrogenation catalysts, and in particular to a hydrogenation catalyst containing a phosphorus-containing alumina carrier, a preparation method thereof, and application of the catalyst in hydrocarbon oil hydrogenation reactions, especially in hydrogenation treatment of wax oil fractions. Background Art

[0002] The increasing environmental awareness and increasingly stringent environmental regulations have forced the oil refining industry to pay more attention to the development of clean fuel production technology. In the future, the market for automotive fuels will tend to be "ultra-low sulfur", and fuels that do not meet emission standards will not be able to enter the market. As an effective desulfurization method, hydrogenation technology plays an increasingly important role in the production of clean automotive fuels, among which high-efficiency hydrogenation catalysts are the core technology of hydrogenation technology. Therefore, the development of new hydrogenation catalysts with higher activity and selectivity has become one of the most urgent needs of the oil refining industry.

[0003] Alumina, especially γ-alumina, is often used as a carrier for the preparation of catalysts because of its good pore structure, specific surface area and heat stability. The precursor of alumina is hydrated alumina, such as pseudo-boehmite, whose particle size, morphology, crystallinity and impurity content all affect the pore volume, pore distribution, specific surface area and other properties of the alumina carrier. In the prior art, by adjusting the particle size, morphology, crystallinity and other properties of hydrated alumina, people can obtain alumina carriers that meet specific needs.

[0004] Introducing phosphorus into alumina can change the pore structure, surface acidity and thermal stability of the carrier, thereby improving the activity of the hydrogenation catalyst. The prior art records a lot of methods for introducing phosphorus, including introduction during the preparation of alumina, introduction by impregnation and introduction during the molding process, but the performance and activity stability of the catalysts prepared in this way need to be further improved when used in distillate oil hydrodesulfurization.

[0005] Introducing an organic dispersant or complexing agent during the preparation of a hydrogenation catalyst can make the resulting catalyst have better hydrogenation refining performance, but there is a defect that the catalytic activity decreases too quickly, resulting in a short catalyst life. In addition, the amount of active metals used in the hydrogenation catalyst and the ratio between them can also affect the performance of the catalyst to a certain extent. Summary of the invention

[0006] In order to further improve the performance of the hydrogenation catalyst, the inventors of the present invention use a phosphorus-containing alumina carrier with specific infrared characteristics, and control the carbon component content and the ratio of the hydrogenation active metal component in the catalyst, so as to obtain a hydrogenation catalyst with better hydrodesulfurization and hydrodenitrogenation activity and activity stability, and significantly extend the service life of the catalyst, thereby making the present invention. Specifically, the present invention includes the following contents:

[0007] First, the present invention provides a hydrogenation catalyst, which comprises a carrier, a hydrogenation active metal component supported on the carrier, and a carbon component, wherein the hydrogenation metal active component is at least one metal element selected from Group VIB and at least one metal element selected from Group VIII; based on the total amount of the hydrogenation catalyst, the carbon component content in terms of element is 0.03-0.8% by weight, the carrier content is 40-85% by weight, and the hydrogenation active metal component satisfies the following relationship: 0.25≤n(VIB) / n(VIB+VIII)≤0.35, wherein n(VIB) represents the amount of substance of the Group VIB metal element, and n(VIB+VIII) represents the sum of the amounts of substance of the Group VIB metal element and the Group VIII metal element; the carrier is phosphorus-containing alumina, and in the IR spectrum of the phosphorus-containing alumina, (I 3670 +I 3580 ) / (I 3770 +I 3720 ) is 1.9-2.8; among which, I 3670 3670cm -1 At the peak height, I 3580 3580cm -1 At the peak height, I 3770 3770cm -1 At the peak height, I 3720 3720cm -1 The peak is high.

[0008] Secondly, the present invention provides a method for preparing a hydrogenation catalyst, the method comprising the following steps:

[0009] (1) contacting an inorganic aluminum-containing compound solution with an acid or a base to perform a precipitation reaction, or contacting an organic aluminum-containing compound with water to perform a hydrolysis reaction, to obtain phosphorus-containing hydrated aluminum oxide;

[0010] (2) aging the phosphorus-containing hydrated alumina obtained above at a pH of 7-10.5;

[0011] (3) calcining the solid product obtained by aging in step (2) to obtain phosphorus-containing alumina;

[0012] (4) loading a water-soluble salt of a hydrogenation active metal component and an organic complexing agent onto the phosphorus-containing alumina carrier obtained in step (3) by an impregnation method, and then drying and calcining the carrier, wherein the hydrogenation active metal component is at least one metal element selected from Group VIB and at least one metal element selected from Group VIII, and the amount of the water-soluble salt of the hydrogenation active metal component and the organic complexing agent and the calcination conditions are such that, based on the total amount of the finished catalyst, the carbon component content is 0.03-0.8% by weight, the carrier content is 40-85% by weight, and the hydrogenation active metal component satisfies the following relationship: 0.25≤n(VIB) / n(VIB+VIII)≤0.35, wherein n(VIB) represents the amount of the metal element of Group VIB, and n(VIB+VIII) represents the sum of the amounts of the metal element of Group VIB and the metal element of Group VIII;

[0013] The precipitation reaction or the hydrolysis reaction in step (1) is carried out in the presence of a grain growth regulator and a phosphorus-containing compound at a pH of 4-7; the grain growth regulator is a substance that can regulate the growth rate of grains on different crystal planes.

[0014] Finally, the present invention also provides the use of the above hydrogenation catalyst and the hydrogenation catalyst prepared by the above method in hydrocarbon oil hydrogenation reaction.

[0015] Compared with the prior art, the hydrogenation performance of the hydrogenation catalyst provided by the present invention is significantly improved, especially the activity stability of the catalyst is significantly improved, which is conducive to extending the service life of the catalyst. In particular, when applied to wax oil hydrogenation reaction, the effect is more obvious. DETAILED DESCRIPTION

[0016] In order to enable those skilled in the art to better understand the present invention, the specific embodiments of the present invention will be described in detail below, but it should be noted that the endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.

[0017] The hydrogenation catalyst provided by the present invention comprises a carrier, a hydrogenation active metal component supported on the carrier, and a carbon component, wherein the hydrogenation active metal component is at least one metal element selected from Group VIB and at least one metal element selected from Group VIII; based on the total amount of the hydrogenation catalyst, the carbon component content in terms of element is 0.03-0.8% by weight, the carrier content is 40-85% by weight, and the hydrogenation active metal component satisfies the following relationship: 0.25≤n(VIB) / n(VIB+VIII)≤0.35, wherein n(VIB) represents the amount of substance of the Group VIB metal element, and n(VIB+VIII) represents the sum of the amounts of substance of the Group VIB metal element and the Group VIII metal element; the carrier is phosphorus-containing alumina, and in the IR spectrum of the phosphorus-containing alumina, (I 3670 +I 3580 ) / (I 3770 +I 3720 ) is 1.9-2.8; among which, I 3670 3670cm -1 At the peak height, I 3580 3580cm -1 At the peak height, I 3770 3770cm -1 At the peak height, I 3720 3720cm -1 The peak is high.

[0018] In the present invention, the IR spectrum is obtained by measuring the IR spectrum using a Nicolet 870 Fourier infrared spectrometer from Nicolet, USA. Specifically, the sample is pressed into a self-supporting sheet, placed in an infrared cell, treated at 450°C for 3 hours under vacuum conditions, and the infrared spectrum of the sample is measured. -1 Peak height: 3580cm -1 Peak height: 3770cm -1 Peak height: 3720cm -1 The peak height at (I 3670 +I 3580 ) / (I 3770 +I 3720 ) value. Alumina carrier of prior art (I 3670 +I 3580 ) / (I 3770 +I 3720 ) is generally lower than 1.8. Preferably, the phosphorus-containing alumina carrier (I 3670 +I 3580 ) / (I 3770 +I 3720 ) is 2-2.7.

[0019] The present invention has no special requirements for the specific surface area and pore volume of phosphorus-containing alumina. Preferably, the nitrogen adsorption pore volume of the phosphorus-containing alumina is 0.7-1.6 ml / g, the BET nitrogen adsorption specific surface area is 250-380 m2 / g, and the pore diameter is 8-16 nm. The pore diameter refers to the diameter corresponding to the highest point of the pore distribution curve.

[0020] In the phosphorus-containing alumina of the present invention, under preferred conditions, based on the total amount of the phosphorus-containing alumina, the content of Al2O3 is 94-99% by weight, preferably 95-98% by weight; the content of P2O5 is 1-6% by weight, preferably 2-5% by weight.

[0021] According to the present invention, the phosphorus-containing alumina can be obtained by roasting phosphorus-containing pseudo-boehmite. The present invention has no particular limitation on the roasting conditions, preferably, the roasting conditions include: a temperature of 350-1000°C, preferably 500-750°C, and a time of 1-10 hours, preferably 2-6 hours.

[0022] The present invention has no particular limitation on the phosphorus-containing pseudo-boehmite, as long as the phosphorus-containing alumina with a specific structure can be obtained by roasting. Preferably, the phosphorus-containing pseudo-boehmite satisfies h of 1.7≤h≤3, wherein h=D(031) / D(020), the D(031) represents the crystal size of the crystal plane represented by the 031 peak in the XRD spectrum of the pseudo-boehmite crystal grains, and D(020) represents the crystal size of the crystal plane represented by the 020 peak in the XRD spectrum of the pseudo-boehmite crystal grains. The 031 peak refers to the peak with 2θ of 34-43° in the XRD spectrum, and the 020 peak refers to the peak with 2θ of 10-15° in the XRD spectrum, and D=Kλ / (Bcosθ), K is the Scherrer constant, λ is the diffraction wavelength of the target material, B is the half-peak width of the diffraction peak, and 2θ is the position of the diffraction peak. The use of this preferred embodiment is more conducive to improving the activity of the catalyst.

[0023] In the present invention, for different diffraction peaks, B and 2θ are taken as the values ​​of the corresponding peaks. For example, when calculating D(031), D(031)=Kλ / (Bcosθ), wherein B is the half-peak width of the 031 diffraction peak, and 2θ is the position of the 031 diffraction peak; when calculating D(020), D(020)=Kλ / (Bcosθ), wherein B is the half-peak width of the 020 diffraction peak, and 2θ is the position of the 020 diffraction peak. More preferably, the h of the pseudo-boehmite satisfies 1.9≤h≤3, and further preferably satisfies 2.2≤h≤2.8. Within this preferred range, the hydrogenation activity of the obtained catalyst is better.

[0024] Phosphorus-containing alumina obtained by roasting phosphorus-containing pseudo-boehmite with h meeting the above requirements has a specific hydroxyl distribution, which is more conducive to improving the hydrogenation activity of the hydrogenation catalyst prepared by using the phosphorus-containing alumina as a carrier. In the pseudo-boehmite prepared by the prior art, h is generally 0.85-1.65.

[0025] According to the present invention, the relative crystallinity of the phosphorus-containing pseudo-boehmite (based on the commercial SB powder of Condea Company) is generally in the range of 45-77%, preferably in the range of 65-77%.

[0026] In the present invention, the crystal structure of pseudo-boehmite is measured by using a D5005 X-ray diffractometer produced by Siemens, Germany, using CuKα radiation, 44 kV, 40 mA, and a scanning speed of 2° / min.

[0027] In the present invention, the phosphorus-containing pseudo-boehmite contains phosphorus and has a specific crystal structure, so that the hydrogenation catalyst obtained by loading the phosphorus-containing alumina carrier made from the phosphorus-containing pseudo-boehmite with hydrogenation active metal components and carbon components exhibits excellent hydrogenation activity and activity stability.

[0028] The hydrogenation active metal component of the present invention is conventionally selected, the VIB group metal component is Mo and / or W, the VIII group metal component is Co and / or Ni; the carbon component content in terms of elements is 0.04-0.6% by weight, the carrier content is 45-80% by weight, the VIB group metal component is Mo and / or W, the VIII group metal component is Co and / or Ni, and the hydrogenation active metal component satisfies the following relationship: 0.27≤n(VIB) / n(VIB+VIII)≤0.32. In a preferred embodiment, when the atomic ratio of the VIII group metal component to the total hydrogenation active metal component is 0.275-0.315, the obtained hydrogenation catalyst has the best performance, especially when applied to the hydrodesulfurization and hydrodenitrogenation reactions of wax oil fractions, the effect is most significant.

[0029] The hydrogenation catalyst provided by the present invention may also contain any additive that can improve the performance of the hydrogenation catalyst of the present invention, such as a metal additive, a non-metal additive, etc., specifically, it may contain at least one of group IA, IIA, IIIA, IVA, VA, VIIA, IIB, IIIB elements and rare earth metal elements, preferably at least one of boron, fluorine, silicon, sodium, magnesium, lithium, zinc, calcium, potassium, titanium, lanthanum, and cerium. The content of the additive calculated as a single element based on the catalyst does not exceed 10% by weight, preferably 0.5-6% by weight.

[0030] The present invention also provides a method for preparing a hydrogenation catalyst. According to the method of the present invention, the precipitation reaction or the hydrolysis reaction is carried out in the presence of a grain growth regulator and a phosphorus-containing compound at a pH of 4-7, which can not only satisfy the precipitation of phosphorus-containing hydrated alumina, but also maintain a relatively low pH condition to avoid excessively fast growth of pseudo-boehmite grains at high pH, ​​thereby strengthening the joint regulatory effect of phosphorus and growth regulators on pseudo-boehmite growth. The entire process of the generation and aging of hydrated alumina and the grain growth of pseudo-boehmite are carried out in the presence of phosphorus-containing compounds and grain regulators, so that the prepared pseudo-boehmite has a special crystal structure and is particularly suitable for acting as a carrier precursor of a heavy oil hydrogenation catalyst.

[0031] According to a specific embodiment of the present invention, step (1) comprises: contacting an inorganic aluminum-containing compound solution, a phosphorus-containing compound, a grain growth regulator and an acid or a base to carry out a precipitation reaction, or, contacting an organic aluminum-containing compound, a phosphorus-containing compound, a grain growth regulator and water to carry out a hydrolysis reaction; controlling the pH of the precipitation reaction or the hydrolysis reaction to be 4-7.

[0032] According to a preferred embodiment of the present invention, the precipitation reaction or the hydrolysis reaction in step (1) is carried out in the presence of a grain growth regulator and a phosphorus-containing compound at a pH of 4-6.5. Carrying out the precipitation reaction or the hydrolysis reaction at the above preferred pH is more conducive to improving the hydrogenation activity of the prepared hydrogenation catalyst in heavy oil hydrogenation.

[0033] The present invention has no particular limitation on other conditions of the precipitation reaction and the hydrolysis reaction except pH. In the present invention, preferably, the temperature of the precipitation reaction and the hydrolysis reaction is independently 30-90°C.

[0034] In the present invention, the conditions for the precipitation reaction are selected in a wide range. Preferably, the conditions for the precipitation reaction include: a reaction temperature of 40-90°C, and a reaction time of 10-60 minutes. Further preferably, the conditions for the precipitation reaction include: a reaction temperature of 45-80°C, and a reaction time of 10-30 minutes.

[0035] The present invention does not particularly limit the conditions of the hydrolysis reaction, as long as water and the organic aluminum-containing compound are in contact to undergo a hydrolysis reaction to generate hydrated aluminum oxide. The present invention has a wide range of water dosage selection during the hydrolysis reaction, as long as the molar ratio of water to the organic aluminum-containing compound is greater than the stoichiometric ratio. The specific conditions for hydrolysis are well known to those skilled in the art. Preferably, the conditions for the hydrolysis reaction include: a reaction temperature of 40-90°C, preferably 45-80°C, and a reaction time of 2-30 hours, preferably 2-20 hours.

[0036] In the present invention, the grain growth regulator is a substance that can regulate the growth rate of grains on different crystal planes, preferably a substance that can regulate the growth rate of grains on 020 crystal planes and 031 crystal planes. For example, it can be various substances that can have a strong adsorption effect on hydrated alumina; preferably, the grain growth regulator is at least one of polyhydric sugar alcohols and their carboxylates and sulfates; further preferably, the grain growth regulator is selected from at least one of sorbitol, glucose, gluconic acid, gluconate, ribitol, ribonic acid, ribonate and sulfate. The gluconate, ribonate and sulfate can each be their soluble salts, for example, can be one or more of potassium salts, sodium salts and lithium salts.

[0037] In the present invention, there is no particular limitation on the method of adding the grain growth regulator. The grain growth regulator can be added alone, or the grain growth regulator can be mixed with one or more raw materials in advance, and then the raw materials containing the grain growth regulator are reacted.

[0038] The present invention has no particular limitation on the amount of the grain growth regulator. Preferably, in the precipitation reaction, the amount of the grain growth regulator is 1-10% by weight, preferably 1.5-8.5% by weight, and more preferably 2-6% by weight, based on alumina.

[0039] Preferably, in the hydrolysis reaction, the amount of the grain growth regulator used is 1-10% by weight, preferably 1.5-8.5% by weight, and more preferably 2-6% by weight, based on the weight of the organic aluminum-containing compound, calculated as aluminum oxide.

[0040] Unless otherwise specified, in the present invention, the amount of the grain growth regulator is calculated based on the weight of the corresponding aluminum oxide in the organic aluminum-containing compound and the inorganic aluminum-containing compound.

[0041] In the present invention, there is no particular limitation on the method of adding the phosphorus-containing compound. The phosphorus-containing compound (or the phosphorus-containing compound aqueous solution) can be added alone, or the phosphorus-containing compound (or its aqueous solution) can be mixed with one or more raw materials in advance, and then the raw materials containing the phosphorus-containing compound are reacted, as long as the precipitation reaction or hydrolysis reaction is carried out in the presence of the phosphorus-containing compound. The preparation method provided by the present invention can ensure the regulating effect of the phosphorus-containing compound on grain growth.

[0042] The present invention has a wide range of selection for the type of the phosphorus-containing compound, which can be a water-soluble inorganic phosphorus-containing compound. Preferably, the phosphorus-containing compound is selected from at least one of phosphoric acid, ammonium phosphate, ammonium hydrogen phosphate, diammonium hydrogen phosphate, sodium phosphate and potassium phosphate.

[0043] In order to better exert the regulating effect of phosphorus-containing compounds on grain growth, preferably, the amount of the phosphorus-containing compounds is such that the content of P2O5 in the prepared phosphorus-containing alumina is 1-6% by weight, preferably 2-5% by weight, based on the total amount of phosphorus-containing alumina.

[0044] It should be noted that, during the research process, the present invention found that adding a grain growth regulator and a phosphorus-containing compound during the precipitation reaction or the hydrolysis reaction is more conducive to adjusting the growth rate of the grains on the 020 crystal plane and the 031 crystal plane, so that h satisfies 1.7≤h≤3, preferably satisfies 1.9≤h≤3, and more preferably satisfies 2.2≤h≤2.8. Adding a grain growth regulator and a phosphorus-containing compound during the precipitation reaction or the hydrolysis reaction allows the subsequent aging reaction to also be carried out in the presence of the grain growth regulator and the phosphorus-containing compound. Preferably, no additional grain growth regulator and phosphorus-containing compound are added during the aging process.

[0045] According to the preparation method provided by the present invention, in step (1), the inorganic aluminum-containing compound is preferably an aluminum salt and / or an aluminate. Accordingly, the inorganic aluminum-containing compound may also be various aluminum salt solutions and / or aluminate solutions, and the aluminum salt solution may be various aluminum salt solutions, for example, it may be an aqueous solution of one or more of aluminum sulfate, aluminum chloride, and aluminum nitrate. Because of the low price, aluminum sulfate solution and / or aluminum chloride solution are preferred. Aluminum salts may be used alone or in combination of two or more. The aluminate solution is any aluminate solution, such as sodium aluminate solution and / or potassium aluminate solution. Because it is easy to obtain and has a low price, sodium aluminate solution is preferred. Aluminate solutions may also be used alone or in combination. There is no particular limitation on the concentration of the inorganic aluminum-containing compound solution. Preferably, the concentration of the inorganic aluminum-containing compound solution is 20-200 g / L in terms of alumina.

[0046] According to the preparation method provided by the present invention, the organic aluminum-containing compound in step (1) can be at least one of various alkoxy aluminums that can undergo hydrolysis reaction with water to produce hydrated aluminum oxide precipitates, for example, it can be at least one of aluminum isopropoxide, aluminum isobutoxide, triisopropoxyaluminum, tri-tert-butoxyaluminum and aluminum isooctoxide.

[0047] According to the preparation method provided by the present invention, the acid in step (1) can be various proton acids or oxides that are acidic in water medium, for example, it can be at least one of sulfuric acid, hydrochloric acid, nitric acid, carbonic acid, phosphoric acid, formic acid, acetic acid, citric acid and oxalic acid. Preferably, the proton acid is selected from at least one of nitric acid, sulfuric acid and hydrochloric acid. The carbonic acid can be generated in situ by passing carbon dioxide into an aluminum salt solution and / or an aluminate solution. The acid can be introduced in the form of a solution, and the concentration of the acid solution is not particularly limited. Preferably, H +The concentration is 0.2-2 mol / L.

[0048] According to the preparation method provided by the present invention, the base described in step (1) can be a hydroxide or a salt that hydrolyzes in an aqueous medium to make the aqueous solution alkaline. Preferably, the hydroxide is selected from at least one of ammonia water, sodium hydroxide and potassium hydroxide; preferably, the salt is selected from at least one of sodium aluminate, potassium aluminate, ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate, potassium bicarbonate and potassium carbonate. When sodium aluminate and / or potassium aluminate are used as the base, the amount of the grain growth regulator and the phosphorus-containing compound is calculated, and the corresponding amount of aluminum oxide in the sodium aluminate and / or potassium aluminate is also considered.

[0049] Specifically, in order to adjust the pH of the hydrolysis reaction, an acid or a base may be introduced into the hydrolysis reaction. The manner and type of introduction of the acid or the base may be as described above and will not be described in detail herein.

[0050] Among them, the method of precipitating aluminum by controlling the pH of the amount of alkali or acid in the reactants is well known to those skilled in the art and will not be described in detail here.

[0051] The present invention has a wide range of conditions for the aging in step (2), as long as the aging is carried out at a pH of 7-10.5. Since the precipitation reaction or the hydrolysis reaction in step (1) is carried out at a pH of 4-7, it is preferred that a base is introduced before the aging to adjust the pH of the aging reaction. The base can be introduced in the form of a solution, and the concentration of the base solution is not particularly limited, preferably OH - The concentration is 0.2-4 mol / L.

[0052] More preferably, the aging in step (2) is carried out at a pH of 8-10.

[0053] In the present invention, the aging conditions of step (2) are selected in a wide range except for pH. Preferably, the aging temperature is 50-95° C., preferably 55-90° C. The aging time is appropriately selected according to the aging temperature. Preferably, the aging time is 0.5-8 hours, preferably 2-6 hours.

[0054] The present invention also includes separating, washing and drying the aged product after the aging reaction. According to the method provided by the present invention, the separation can be a well-known technique in the art, such as a method of filtering or centrifugal separation. The washing and drying methods can be methods commonly used in the preparation of pseudo-boehmite, for example, the washing agent can be water, and the drying can be at least one of oven drying, forced air drying, spray drying and flash drying. The drying temperature can be 100-350°C, preferably 120-300°C.

[0055] In the preparation method provided by the present invention, there is no particular limitation on the calcination process in step (3). Preferably, the method provided by the present invention further comprises molding the solid product or the phosphorus-containing aluminum oxide before or after the calcination. Preferably, the solid product obtained by aging in step (2) is molded and dried, and then the calcination is performed, and the molding is preferably extrusion molding. In order to ensure that the molding is carried out smoothly, water, an extrusion aid and / or an adhesive may be added to the solid product obtained by aging in step (2), and a pore expander may be optionally added. The types and amounts of the extrusion aid, peptizing agent and pore expander are well known to those skilled in the art; for example, a common extrusion aid may be selected from at least one of sesbania powder, methyl cellulose, starch, polyvinyl alcohol and polyethanol, the peptizing agent may be an inorganic acid and / or an organic acid, and the pore expander may be at least one of starch, synthetic cellulose, a polyol and a surfactant. The synthetic cellulose is preferably at least one of hydroxymethyl cellulose, methyl cellulose, ethyl cellulose and hydroxycellulose fatty alcohol polyvinyl ether; the polymeric alcohol is preferably at least one of polyethylene glycol, polypropylene glycol and polyvinyl alcohol; the surfactant is preferably at least one of fatty alcohol polyvinyl ether, fatty alcohol amide and its derivatives, propylene alcohol copolymer with a molecular weight of 200-10000 and maleic acid copolymer. The drying conditions in step (3) preferably include: the drying temperature can be 40-350°C, more preferably 100-200°C; the drying time can be 1-24 hours, more preferably 2-12 hours.

[0056] In the preparation method provided by the present invention, there is no particular limitation on the calcination conditions in step (3). Preferably, the calcination conditions in step (3) include: a temperature of 350-1000°C, preferably 400-800°C, and a time of 1-10 hours, preferably 2-6 hours.

[0057] According to the method of the present invention, the hydrogenation active metal component in the preparation method is conventionally selected, the VIB group metal component is Mo and / or W, and the VIII group metal component is Co and / or Ni; the molar ratio of the organic complexing agent to the hydrogenation active metal component is 0.03-2:1, preferably 0.08-1.5:1; the amount of each component is such that the carbon component content in the final hydrogenation catalyst is 0.04-0.6% by weight in terms of element, the carrier content is 45-80% by weight, and the hydrogenation active metal component satisfies the following relationship: 0.27≤n(VIB) / n(VIB+VIII)≤0.32, and the hydrogenation active metal component content in terms of oxide is 20-50% by weight. In another preferred embodiment, when the amount of each component added is such that the atomic ratio of the VIII group metal component to the total hydrogenation active metal component is 0.275-0315, the obtained hydrogenation catalyst has the best performance, especially when applied to the hydrodesulfurization and hydrodenitrogenation reactions of wax oil fractions, the effect is most significant.

[0058] The inventors of the present invention have further discovered through research that adding an organic complexing agent during the impregnation process and converting it into a specific content of carbon through roasting can not only improve the activity of the catalyst, but also effectively maintain the high activity of the catalyst for a long time, thereby greatly improving the service life of the catalyst. It is speculated that the reason may be that the organic complexing agent added during the impregnation process hinders the aggregation of active metals during the roasting process, making them more evenly dispersed; roasting after impregnation can convert metal compounds into metal oxides and convert organic complexing agents into carbon, thereby making the combination between active metals and carriers more firm, improving the activity and stability of the catalyst. Therefore, this technology can effectively solve the technical defects of conventional impregnation methods and existing complex impregnation methods.

[0059] According to the present invention, based on the total amount of the finished catalyst, the carbon component content in the finished catalyst is preferably 0.04-0.6% by weight; in order to achieve this content, the roasting conditions of step (4) of the present invention are further limited, and the above carbon content can be obtained by controlling the roasting temperature and the amount of combustion-supporting gas introduced in the roasting conditions, and the combustion-supporting gas can be various gases with an oxygen content of not less than 20% by volume, such as one or more of air, oxygen and their mixed gases. The amount of the combustion-supporting gas introduced is not less than 0.2 liters / gram·hour. The introduction of the combustion-supporting gas, on the one hand, meets the combustion conditions, so that the salt of the active metal component is converted into oxides, and the organic complexing agent is converted into carbon; on the other hand, the carbon dioxide and water and other components formed by the combustion can be discharged to avoid deposition on the catalyst to cause vacancy obstruction to the active phase. Preferably, the amount of gas introduced is 0.2-20 liters / (gram·hour), more preferably 0.3-10 liters / (gram·hour). The "gram" here represents the weight of the carrier.

[0060] According to the present invention, the calcination temperature is 350-500°C, preferably 360-450°C, and the calcination time is 0.5-8h, preferably 1-6h. Controlling the calcination temperature within the above range can ensure that the organic complexing agent can form carbon on the carrier within the above content range to obtain a finished catalyst.

[0061] In the present invention, the organic complexing agent is selected from one or more oxygen-containing and / or nitrogen-containing organic substances. The oxygen-containing organic substance is preferably selected from one or more organic alcohols and organic acids. The organic alcohol is preferably a polyol with a divalent or higher valence, and is further preferably a polyol with a carbon number of 2-6 or its oligomer or polymer, such as one or more of ethylene glycol, propylene glycol, polyethylene glycol, diethylene glycol, and butanediol. The molecular weight of the polyethylene glycol is preferably 200-1500. The organic acid is preferably a C2-C7 compound containing one or more COOH groups, and can specifically be one or more of acetic acid, maleic acid, oxalic acid, aminotriacetic acid, 1,2-cyclohexanediaminetetraacetic acid, citric acid, tartaric acid, and malic acid. The nitrogen-containing organic substance is preferably selected from one or more organic amines and organic ammonium salts. The organic amine is preferably a C2-C7 compound containing one or more NH groups, and can be a primary amine, a secondary amine, or a tertiary amine, and is particularly preferably ethylenediamine. The organic ammonium salt is preferably EDTA.

[0062] Specifically, the present invention particularly preferably said organic complexing agent is one or more of ethylene glycol, glycerol, polyethylene glycol (molecular weight is preferably 200-1500), diethylene glycol, butanediol, acetic acid, maleic acid, oxalic acid, aminotriacetic acid, 1,2-cyclohexanediaminetetraacetic acid, citric acid, tartaric acid, malic acid, ethylenediamine and EDTA. Preferably said organic complexing agent is selected from one or more of organic acids, more preferably, said organic complexing agent is selected from one or more of C2-C7 fatty acids. Using organic acids as organic complexing agents can obtain hydrogenation catalysts with higher activity.

[0063] The present invention has no particular limitation on the drying conditions, and may be various drying conditions commonly used in the art. The drying conditions are preferably a drying temperature of 100-250° C. and a drying time of 1-12 h.

[0064] According to the use of the hydrogenation catalyst provided by the present invention in the hydrogenation reaction of hydrocarbon oil, the hydrocarbon oil is the hydrogenation catalyst provided by the present invention, or the hydrogenation catalyst prepared by the method of the present invention.

[0065] The catalyst of the present invention is suitable for use in refining processes such as hydrodesulfurization and hydrodenitrogenation of various hydrocarbon oil raw materials. The hydrocarbon oil raw materials may be gasoline, diesel, lubricating oil, kerosene and naphtha, or atmospheric residue, vacuum residue, petroleum wax and Fischer-Tropsch synthetic oil, and are particularly suitable for wax oil fractions.

[0066] The conditions of the hydrogenation reaction of the present invention are not particularly limited and can be selected conventionally in the art. Generally, the conditions of the hydrogenation refining include: the temperature can be 300-400°C; the pressure can be 1.0-8.0 MPa in gauge pressure; the liquid hourly volume space velocity can be 0.5-3.0 hours -1 , the hydrogen to oil volume ratio can be 100-700.

[0067] The catalyst provided by the present invention is preferably vulcanized by conventional methods in the art before use. Generally, the vulcanization conditions may include: pre-sulfurization for 2-4 hours with one or more of sulfur, hydrogen sulfide, carbon disulfide, dimethyl disulfide or other sulfur-containing raw materials at a temperature of 180-450° C. in the presence of hydrogen. The pre-sulfurization may be performed outside the reactor or in situ in the reactor.

[0068] The implementation process of the present invention and the beneficial effects produced are described in detail below through specific embodiments, but they do not constitute any limitation on the implementation scope of the present invention.

[0069] In the following examples, the content of each element in the catalyst was analyzed and determined using a 3271E X-ray fluorescence spectrometer produced by Rigaku Corporation of Japan. The carbon content in the semi-finished catalyst was analyzed and determined using an EMIA-320V carbon-sulfur analyzer produced by HORIBA of Japan. XRD was measured on a SIMENS D5005 X-ray diffractometer, CuKα radiation, 44 kV, 40 mA, and a scanning speed of 2° / min. According to the Scherrer formula: D=Kλ / (Bcosθ) (D is the grain size, λ is the diffraction wavelength of the target material, B is the half-peak width of the corrected diffraction peak, and 2θ is the position of the diffraction peak), the grain size of (020) is calculated as D(020) with 2θ as the peak parameter of 10-15°, and the grain size of (031) is calculated as D(031) with 2θ as the peak parameter of 34-43°, and h=D(031) / D(020) is calculated.

[0070] The IR spectrum is obtained by using a Nicolet 870 Fourier infrared spectrometer from Nicolet, USA. Specifically, the sample is pressed into a self-supporting sheet, placed in an infrared cell, treated at 450°C for 3 hours under vacuum conditions, and the infrared spectrum of the sample is measured. -1 Peak height: 3580cm -1Peak height: 3770cm -1 Peak height: 3720cm -1 The value of m is calculated from the peak height at 3670 +I 3580 ) / (I 3770 +I 3720 ) value.

[0071] In the following examples, all raw materials involved are commercially available unless otherwise specified.

[0072] Example 1

[0073] This example is used to illustrate the hydrogenation catalyst and its preparation method provided by the present invention.

[0074] In a 2-liter reaction tank, 5000 ml of an aluminum sulfate solution with a concentration of 60 g aluminum oxide / L, 6.0 g ribitol, 8.0 mL of 85 wt% concentrated phosphoric acid, and a 6 wt% ammonia solution were added in parallel for precipitation reaction. The reaction temperature was 50°C and the reaction time was 30 minutes. The flow rate of the ammonia solution was controlled to make the pH of the reaction system 5.0. After the precipitation reaction was completed, an appropriate amount of ammonia water was added to the slurry to make the pH of the slurry 8.7. The slurry was aged at 70°C for 120 minutes and then filtered. The filter cake was pulped and washed twice with deionized water. The filter cake was dried at 120°C for 24 hours to obtain hydrated alumina PA1. XRD characterization showed that PA1 had a pseudo-boehmite structure.

[0075] The h value of PA1 calculated by XRD characterization is listed in Table 1. The relative crystallinity of PA1 and the content of P2O5 are also listed in Table 1. After calcination at 600°C for 4 hours, the hydroxyl groups on the surface of phosphorus-containing alumina were measured by infrared spectroscopy, and the calculated m value is listed in Table 1.

[0076] 1000 g of PA1 and 30 g of sesbania powder (produced by Jiangsu Fengxian Runshun Trading Co., Ltd.) were mixed evenly, and then 920 ml of an aqueous solution containing 28 g of nitric acid was added for mixing, and then extruded into butterfly-shaped wet strips with an outer diameter of 1.7 mm on a plunger extruder, and the butterfly-shaped wet strips were dried at 120° C. for 4 hours, and then calcined at 600° C. for 3 hours to obtain carrier Z1. The content of P2O5 in carrier Z1, as well as its pore volume, specific surface area and pore diameter are listed in Table 2.

[0077] 54 g of molybdenum trioxide, 21 g of basic nickel carbonate, 13 g of phosphoric acid, and 30 g of citric acid were weighed and put into 200 g of deionized water, heated and stirred to dissolve to obtain a clear impregnation solution, and 200 g of the phosphorus-containing alumina carrier prepared in Example 1 was impregnated with the above solution by saturated impregnation method for 2 hours, then dried at 150° C. for 2 hours, and then calcined under the condition of passing air flow, the calcination temperature was 360° C., the time was 3 hours, and the air-to-agent ratio was 10 liters / (g·hour), to obtain the finished catalyst S1. Based on the total amount of S1, the content of each component in the hydrogenation catalyst S1 and the ratio of the hydrogenation metal active component are shown in Table 3.

[0078] Comparative Example 1

[0079] The carrier DZ1 and the hydrogenation catalyst DS1 were prepared according to the method of Example 1, except that only 8.0 mL of phosphoric acid with a concentration of 85 wt% was added to the aluminum sulfate solution without ribitol, to obtain hydrated alumina CPA1. XRD characterization was performed according to the method of Example 1. CPA1 has a pseudo-boehmite structure. The h value of CPA1 calculated by XRD characterization is listed in Table 1, and the relative crystallinity and P2O5 content are also listed in Table 1. After calcination at 600°C for 4 hours, the hydroxyl groups on the surface of phosphorus-containing alumina were measured by infrared spectroscopy, and the calculated m values ​​are listed in Table 1. The pore volume, specific surface area and pore diameter of the carrier DZ1 are listed in Table 2. Based on the total amount of DS1, the content of each component in the hydrogenation catalyst DS1 and the proportion of hydrogenation metal active components are shown in Table 3.

[0080] Comparative Example 2

[0081] The carrier DZ2 and hydrogenation catalyst DS2 were prepared according to the method of Example 1, except that the flow rate of the ammonia solution was directly controlled to make the pH of the reaction system 8.7. After the precipitation reaction was completed, it was not necessary to add ammonia solution to the slurry to adjust the pH value, and hydrated alumina CPA2 was obtained. According to the method of Example 1, XRD characterization was performed. CPA2 has a pseudo-boehmite structure. The h value of CPA2 calculated by XRD characterization is listed in Table 1, and the relative crystallinity and P2O5 content are also listed in Table 1. After calcination at 600°C for 4 hours, the hydroxyl groups on the surface of phosphorus-containing alumina were measured by infrared spectroscopy, and the calculated m value is listed in Table 1. The content of P2O5 in the carrier DZ2, as well as its pore volume, specific surface area and pore diameter are listed in Table 2. Based on the total amount of DS2, the content of each component in the hydrogenation catalyst DS2 and the proportion of hydrogenation metal active components are shown in Table 3.

[0082] Comparative Example 3

[0083] The carrier DZ3 and the hydrogenation catalyst DC3 were prepared according to the method of Example 1, except that only 6.0 grams of ribitol was added to the aluminum sulfate solution without concentrated phosphoric acid to obtain hydrated alumina CPA3. According to the method of Example 1, XRD characterization was used. CPA3 has a pseudo-boehmite structure. The h value of CPA3 calculated by XRD characterization is listed in Table 1, and the relative crystallinity and P2O5 content are also listed in Table 1. After calcination at 600°C for 4 hours, the hydroxyl groups on the surface of alumina were measured by infrared spectroscopy, and the calculated m values ​​are listed in Table 1. The content of P2O5 in the carrier DZ3, as well as its pore volume, specific surface area and pore diameter are listed in Table 2. Based on the total amount of DS3, the content of each component in the hydrogenation catalyst DS3 and the proportion of hydrogenation metal active components are shown in Table 3.

[0084] Comparative Example 4

[0085] The catalyst was prepared by using the carrier of Example 1 and the method for preparing the hydrogenation catalyst in Example 1, except that no citric acid was added in the preparation of the impregnation solution. The obtained catalyst was DS4. Based on the total amount of DS4, the content of each component in the hydrogenation catalyst DS4 and the ratio of the hydrogenation metal active component are shown in Table 3.

[0086] Comparative Example 5

[0087] The carrier of Example 1 was used to prepare the hydrogenation catalyst DS5, the only difference being the amount of hydrogenation active metal used, specifically: 54.5 grams of molybdenum trioxide, 19 grams of basic nickel carbonate, 13 grams of phosphoric acid, and 30 grams of citric acid were put into 200 grams of deionized water, heated and stirred to dissolve to obtain a clear impregnation solution, and the above solution was used to impregnate 200 grams of the phosphorus-containing alumina carrier prepared in Example 1 by a saturated impregnation method, and the remaining steps and conditions were the same to obtain the finished catalyst DS5. Based on the total amount of DS5, the content of each component in the hydrogenation catalyst DS5 and the ratio of the hydrogenation metal active component are shown in Table 3.

[0088] Example 2

[0089] This example is used to illustrate the hydrogenation catalyst and its preparation method provided by the present invention.

[0090] In a 2-liter reaction tank, 4000 ml of an aluminum chloride solution containing 22.1 mL of 85 wt% concentrated phosphoric acid and 4.52 g / L of sorbitol and 1000 ml of a sodium aluminate solution containing 210 g of aluminum oxide / L and a caustic coefficient of 1.58 were added in parallel to carry out a precipitation reaction. The reaction temperature was 80° C., the flow rate of the reactants was adjusted so that the neutralization pH value was 4.0, and the reaction residence time was 15 minutes; 5 wt% dilute ammonia water was added to the resulting slurry to adjust the slurry pH to 9.0, and the temperature was raised to 85° C., aged for 3 hours, and then filtered with a vacuum filter. After the filtration was completed, 20 liters of deionized water (temperature 85° C.) were added to the filter cake to rinse the filter cake for about 30 minutes. The washed qualified filter cake was added into 3.0 liters of deionized water and stirred into slurry. The slurry was pumped into a spray dryer for drying. The outlet temperature of the spray dryer was controlled in the range of 100-110°C. The material drying time was about 2 minutes. After drying, hydrated alumina PA2 was obtained. According to the method of Example 1, PA2 was characterized by XRD. PA2 had a pseudo-boehmite structure. The h value of PA2 calculated by XRD characterization was listed in Table 1. The relative crystallinity and P2O5 content were also listed in Table 1. After calcination at 600°C for 4 hours, the hydroxyl group on the surface of phosphorus-containing alumina was measured by infrared spectroscopy, and the calculated m value was listed in Table 1.

[0091] The carrier Z2 was prepared according to the method of Example 1, except that the PA2 was used instead of PA1, and the calcination temperature was 650° C. The content of P2O5 in the carrier Z2, as well as its pore volume, specific surface area and pore diameter are listed in Table 2.

[0092] 54 g of molybdenum trioxide, 23 g of basic nickel carbonate, 13 g of phosphoric acid and 30 g of citric acid were weighed respectively and put into 200 g of deionized water, heated and stirred to dissolve to obtain a clarified impregnation solution, and 200 g of the phosphorus-containing alumina carrier prepared in Example 1 was impregnated with the above solution by a saturated impregnation method for 2 hours. Then, it was dried at 150°C for 2 hours, and then calcined under a flow of air at a temperature of 400°C for 2 hours. The gas-to-agent ratio was 2 liters / (g·hour) to obtain a finished catalyst S2. Based on the total amount of S2, the content of each component in the hydrogenation catalyst S2 and the proportion of the hydrogenation metal active component are shown in Table 3.

[0093] Example 3

[0094] This example is used to illustrate the hydrogenation catalyst and its preparation method provided by the present invention.

[0095] In a 2-liter three-necked flask with a stirrer and a reflux condenser, 1000 g of an azeotropic mixture of isopropanol and water (water content is 15 wt%), 4.6 mL of 85% concentrated phosphoric acid, 15 g of ribose acid, and ammonia water are added to adjust the pH to 5.1, and then heated to 60° C., 500 g of molten aluminum isopropoxide is slowly dripped into the flask through a separatory funnel, reacted for 2 hours, ammonia water is added to adjust the pH to 8.5, refluxed for 20 hours, dehydrated isopropanol is evaporated, aged at 80° C. for 6 hours, and water-containing isopropanol is evaporated while aging. After aging, the aged hydrated alumina is filtered and dried at 120° C. for 24 hours to obtain hydrated alumina PA3. According to the method of Example 1, PA3 has a pseudo-boehmite structure, and the h value of PA3 calculated by XRD characterization is listed in Table 1, and the relative crystallinity and P2O5 content are also listed in Table 1. After calcination at 600°C for 4 hours, the hydroxyl groups on the surface of phosphorus-containing alumina were measured by infrared spectroscopy, and the calculated m values ​​are listed in Table 1.

[0096] Using the method of Example 1, 1000 g of PA3 was used to prepare carrier Z3. The content of P2O5 in Z3 as well as its pore volume, specific surface area and pore diameter are listed in Table 2.

[0097] 60 g of molybdenum trioxide, 28 g of basic nickel carbonate, 15 g of phosphoric acid, and 30 g of citric acid were weighed and put into 200 g of deionized water, heated and stirred to dissolve to obtain a clear impregnation solution, and 200 g of the phosphorus-containing alumina carrier prepared in Example 1 was impregnated with the above solution by saturated impregnation method for 2 hours, then dried at 150°C for 2 hours, and then calcined under the condition of passing air flow, the calcination temperature was 400°C, the time was 2 hours, and the air-to-agent ratio was 2 liters / (g·hour), to obtain the finished catalyst S3. Based on the total amount of S3, the content of each component in the hydrogenation catalyst S3 and the ratio of the hydrogenation metal active component are shown in Table 3.

[0098] Table 1

[0099]

[0100] Note: m means (I 3670 +I 3580 ) / (I 3770 +I 3720 )

[0101] Table 2

[0102]

[0103] Table 3

[0104]

[0105] From the results in Table 1, it can be seen that the phosphorus-containing pseudo-boehmite prepared by the method provided by the present invention has the characteristic of 1.7≤h≤3, preferably 2.2≤h≤2.8, while the h values ​​of various pseudo-boehmites prepared by the methods of the prior art and the methods in the comparative examples are all less than 1.7. In the IR characterization spectrum of aluminum oxide obtained by calcining the phosphorus-containing pseudo-boehmite prepared by the method of the present invention at 600°C, the hydroxyl group has the characteristic (I 3670 +I 3580 ) / (I 3770 +I 3720 ) is 1.9-2.8, preferably 2-2.7, and the pseudo-boehmite prepared by the prior art method and the method in the comparative example, after being calcined at 600°C, the IR characterization spectrum of alumina obtained has the hydroxyl characteristic (I 3670 +I 3580 ) / (I 3770 +I 3720 )<1.8.

[0106] Evaluation example

[0107] In this test example, the desulfurization activity and denitrification activity of the hydrotreating catalyst prepared by the method provided by the present invention and the hydrotreating catalyst provided by the comparative example were evaluated according to the following method. Qingdao wax oil was used as the raw material, and its properties were as follows:

[0108]

[0109] The desulfurization and denitrification activities of the catalyst were evaluated on a 120 ml wax oil hydrogenation unit. The catalyst needs to be pre-sulfurized before the reaction. The catalyst is loaded with 100 mL. The pre-sulfurization conditions are: 6.4 MPa, 290 ° C, 4 h, hydrogen-oil volume ratio 300:1, and the sulfide oil feed rate is 150 mL / h. The reaction conditions are: hydrogen partial pressure 8.0 MPa, reaction temperature 355 ° C, hydrogen-oil volume ratio 800, liquid hourly space velocity 1.4 h -1 Samples were taken on the 2nd and 12th day after the reaction, and the sulfur and nitrogen contents in the raw materials and products of the hydrodesulfurization and hydrodenitrogenation reactions were determined by gas chromatography.

[0110] The relative hydrodesulfurization activity of the reference agent DS1 was used to evaluate the hydrodesulfurization activity of the catalyst. The hydrodesulfurization reaction was treated as a 1.65-order reaction and the reaction rate constant k(X) of catalyst X was calculated according to formula (1): HDS :

[0111]

[0112] In formula (1), LHSV is the liquid hourly space velocity of the hydrocarbon oil during the hydrotreating reaction.

[0113] The hydrodesulfurization activity of catalyst DS1 [denoted as k(D1) HDS ] as the benchmark, the relative hydrodesulfurization activity of catalyst X was calculated according to formula (2):

[0114]

[0115] The relative hydrodenitrogenation activity relative to the reference agent DS1 was used to evaluate the hydrodenitrogenation activity of the catalyst. The hydrodesulfurization reaction was treated as a first-order reaction and the reaction rate constant k(X) of catalyst X was calculated according to formula (3): HDN :

[0116]

[0117] In formula (1), LHSV is the liquid hourly space velocity of the hydrocarbon oil during the hydrotreating reaction.

[0118] The hydrodenitrogenation activity of catalyst DS1 [denoted as k(D1) HDN ] as the benchmark, the relative hydrodenitrogenation activity of catalyst X was calculated according to formula (4):

[0119]

[0120] The hydrotreating evaluation results of the catalysts prepared in the examples and comparative examples are shown in Table 4.

[0121] The sulfur content in the oil sample is determined by the coulometry method (for specific methods, see petrochemical analysis method RIPP62-90). The nitrogen content in the oil sample is determined by the chemiluminescence method (for specific methods, see petrochemical analysis method RIPP SH0704-Z).

[0122] The results in Table 4 show that, compared with the hydrogenation catalyst prepared by the existing method, the catalyst provided by the present invention has significantly improved hydrodesulfurization activity, and the hydrodenitrogenation activity is also improved. In addition, by comparing the data of the relative hydrodesulfurization activity and the relative hydrodenitrogenation activity on the 12th day of the reaction in Table 4, it can be seen that the activity of the catalyst provided by the present invention is significantly improved relative to the comparative example D1 for a long time reaction. Therefore, the catalyst prepared by the method provided by the present invention significantly extends the service life of the catalyst, and the effect is remarkable.

[0123] Table 4

[0124]

[0125] Note: In Table 4, “-” means no test was performed.

[0126] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0127] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. In addition, the various different embodiments of the present invention can also be combined arbitrarily, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A hydrogenation catalyst, comprising a carrier, a hydrogenation active metal component supported on the carrier, and a carbon component, wherein the hydrogenation active metal component is at least one metal element selected from Group VIB and at least one metal element selected from Group VIII; based on the total amount of the hydrogenation catalyst, the carbon component content in terms of element is 0.03-0.8% by weight, the carrier content is 40-85% by weight, and the hydrogenation active metal component satisfies the following relationship: 0.27≤n(VIB) / n(VIB+VIII)≤0.32, wherein n(VIB) represents the amount of substance of the Group VIB metal element, and n(VIB+VIII) represents the sum of the amounts of substance of the Group VIB metal element and the Group VIII metal element; the carrier is phosphorus-containing alumina, and in the IR spectrum of the phosphorus-containing alumina, (I 3670 +I 3580 ) / (I 3770 +I 3720 ) is 2-2.7; among them, I 3670 3670 cm -1 At the peak height, I 3580 3580 cm -1 At the peak height, I 3770 3770 cm -1 At the peak height, I 3720 3720 cm -1 Based on the total amount of the phosphorus-containing aluminum oxide, the content of Al2O3 is 94-99% by weight, and the content of P2O5 is 1-6% by weight.

2. The hydrogenation catalyst according to claim 1, wherein The carbon component content is 0.04-0.6% by weight, the carrier content is 45-80% by weight, the VIB group metal component is Mo and / or W, and the VIII group metal component is Co and / or Ni.

3. The hydrogenation catalyst according to claim 1, wherein The nitrogen adsorption pore volume of the phosphorus-containing alumina is 0.7-1.6 ml / g, the BET nitrogen adsorption specific surface area is 250-380 m2 / g, and the pore diameter is 8-16 nm; based on the total amount of the phosphorus-containing alumina, the Al2O3 content is 95-98% by weight; and the P2O5 content is 2-5% by weight.

4. The hydrogenation catalyst according to claim 1, wherein The phosphorus-containing alumina is obtained by calcining phosphorus-containing pseudo-boehmite; The phosphorus-containing pseudo-boehmite h Satisfy 1.7≤ h ≤3, where h =D(031) / D(020), wherein D(031) represents the grain size of the crystal plane represented by the 031 peak in the XRD spectrum of the pseudo-boehmite grains, and D(020) represents the grain size of the crystal plane represented by the 020 peak in the XRD spectrum of the pseudo-boehmite grains. The 031 peak refers to the peak with 2θ of 34-43° in the XRD spectrum, and the 020 peak refers to the peak with 2θ of 10-15° in the XRD spectrum. D=Kλ / (Bcosθ), K is the Scherrer constant, λ is the diffraction wavelength of the target material, B is the half-width of the diffraction peak, and 2θ is the position of the diffraction peak.

5. The hydrogenation catalyst according to claim 4, wherein The pseudo-boehmite h Satisfy 1.9≤ h ≤3; the relative crystallinity of the phosphorus-containing pseudo-boehmite is 45-77%.

6. The hydrogenation catalyst according to claim 5, wherein The pseudo-boehmite h Satisfy 2.2≤ h ≤2.

8.

7. A method for preparing the hydrogenation catalyst according to claim 1, comprising the steps of: (1) contacting an inorganic aluminum-containing compound solution with an acid or a base to carry out a precipitation reaction, or contacting an organic aluminum-containing compound with water to carry out a hydrolysis reaction, to obtain phosphorus-containing hydrated aluminum oxide; (2) aging the phosphorus-containing hydrated alumina obtained above at a pH of 7-10.5; (3) calcining the solid product obtained by aging in step (2) to obtain phosphorus-containing alumina; (4) using an impregnation method to load a water-soluble salt of a hydrogenation active metal component, phosphoric acid and an organic complexing agent onto the phosphorus-containing alumina carrier obtained in step (3), and then drying and calcining the carrier, wherein the hydrogenation active metal component is at least one metal element selected from Group VIB and at least one metal element selected from Group VIII, and the amount of the water-soluble salt of the hydrogenation active metal component and the organic complexing agent and the calcination conditions are such that, based on the total amount of the finished catalyst, the carbon component content is 0.03-0.8% by weight, the carrier content is 40-85% by weight, and the hydrogenation active metal component satisfies the following relationship: 0.27≤n(VIB) / n(VIB+VIII)≤0.32, wherein n(VIB) represents the amount of the metal element of Group VIB, and n(VIB+VIII) represents the sum of the amounts of the metal element of Group VIB and the metal element of Group VIII; The precipitation reaction or the hydrolysis reaction in step (1) is carried out in the presence of a grain growth regulator and a phosphorus-containing compound at a pH of 4-7; the grain growth regulator is a substance that can regulate the growth rate of grains on different crystal planes; the temperature of the precipitation reaction and the hydrolysis reaction is independently 30-90°C.

8. The preparation method according to claim 7, wherein: The precipitation reaction or the hydrolysis reaction in step (1) is carried out in the presence of a grain growth regulator and a phosphorus-containing compound at a pH of 4-6.5; The conditions of the precipitation reaction include: the reaction temperature is 40-90° C., and the reaction time is 10-60 minutes; the conditions of the hydrolysis reaction include: the reaction temperature is 40-90° C., and the reaction time is 2-30 hours.

9. The preparation method according to claim 7, wherein: The conditions of the precipitation reaction include: the reaction temperature is 45-80° C., and the reaction time is 10-30 minutes; the conditions of the hydrolysis reaction include: the reaction temperature is 45-80° C., and the reaction time is 2-20 hours.

10. The preparation method according to claim 7, wherein: The grain growth regulator is a substance that can regulate the growth rate of grains on the 020 crystal plane and the 031 crystal plane; In the precipitation reaction, the amount of the grain growth regulator is 1-10% by weight of the inorganic aluminum-containing compound, calculated as aluminum oxide; Calculated on the basis of aluminum oxide, in the hydrolysis reaction, the amount of the grain growth regulator used is 1-10% by weight of the weight of the organic aluminum-containing compound.

11. The preparation method according to claim 10, wherein: In the precipitation reaction, the amount of the grain growth regulator is 1.5-8.5% by weight of the inorganic aluminum-containing compound, calculated as aluminum oxide; Calculated on the basis of aluminum oxide, in the hydrolysis reaction, the amount of the grain growth regulator used is 1.5-8.5% by weight of the organic aluminum-containing compound.

12. The preparation method according to claim 7, wherein: The phosphorus-containing compound is selected from at least one of phosphoric acid, ammonium phosphate, ammonium hydrogen phosphate, diammonium hydrogen phosphate, sodium phosphate and potassium phosphate; the amount of the phosphorus-containing compound is such that the content of P2O5 in the prepared phosphorus-containing alumina is 1-6% by weight, based on the total amount of the phosphorus-containing alumina.

13. The preparation method according to any one of claims 7 to 12, wherein: The aging in step (2) is carried out at a pH of 8-10 and a temperature of 50-95°C; Aging time is 0.5-8 hours; The calcination conditions in step (3) include: a temperature of 350-1000° C. and a time of 1-10 hours.

14. The preparation method according to claim 13, wherein: The calcination conditions in step (3) include: a temperature of 400-800° C. and a time of 2-6 hours.

15. The preparation method according to any one of claims 7 to 12, wherein: The inorganic aluminum-containing compound is an aluminum salt and / or aluminate; the organic aluminum-containing compound is at least one of alkoxy aluminums that can undergo a hydrolysis reaction with water to produce a hydrated aluminum oxide precipitate; the acid is at least one of sulfuric acid, hydrochloric acid, nitric acid, carbonic acid, phosphoric acid, formic acid, acetic acid, citric acid and oxalic acid; and the base is at least one of sodium hydroxide, potassium hydroxide and ammonia water.

16. The preparation method according to any one of claims 7 to 12, wherein:The VIB group metal component is Mo and / or W, and the VIII group metal component is Co and / or Ni; the molar ratio of the organic complexing agent to the hydrogenation active metal component is 0.03-2:1; the dosage of each component is such that in the final hydrogenation catalyst, the carbon component content calculated as element is 0.04-0.6% by weight, the carrier content is 45-80% by weight, and the hydrogenation active metal component content calculated as oxide is 20-50% by weight.

17. The preparation method according to any one of claims 7 to 12, wherein: The organic complexing agent is selected from one or more oxygen-containing and / or nitrogen-containing organic substances, the oxygen-containing organic substance is selected from one or more organic alcohols and organic acids, and the nitrogen-containing organic substance is selected from one or more organic amines and organic ammonium salts.

18. The preparation method according to any one of claims 7 to 12, wherein: The organic complexing agent is one or more organic acids having 2 to 7 carbon atoms.

19. The preparation method according to claim 7, wherein: The calcination in step (4) is carried out under the condition of introducing gas, and the calcination temperature is 350-500°C, the calcination time is 0.5-8h, and the gas introduction amount is 0.2-20 liters / (g·hour).

20. The preparation method according to claim 19, wherein: The calcination temperature is 360-450° C., the calcination time is 1-6 hours, and the gas introduction amount is 0.3-10 liters / (g·hour).

21. Use of the hydrogenation catalyst according to any one of claims 1 to 6 or the hydrogenation catalyst prepared by the preparation method according to any one of claims 7 to 20 in hydrocarbon oil hydrogenation reaction.