Regeneration method of catalyst to be regenerated and activity recovery method of catalyst to be regenerated

Through the combination of programmed temperature oxidation method and staged roasting, combined with the contact treatment of organic alcohol compounds and carboxylic acid compounds, the problem of incomplete or excessive roasting during hydrogenation catalyst regeneration is solved, and the activity recovery effect of the catalyst is significantly improved.

CN116060053BActive Publication Date: 2024-10-11CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111274373.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-11
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

In existing hydrogenation catalyst regeneration methods, high-temperature roasting can easily lead to incomplete roasting or excessive roasting, which makes it difficult to effectively restore catalyst activity and has poor control over catalysts with special pore structures.

Method used

The programmed temperature oxidation method is used to determine the peak results of the substances to be removed, and the temperature is increased and roasted in stages, and the regenerated catalyst is contacted with organic alcohol compounds and/or carboxylic acid compounds for drying to restore its activity.

Benefits of technology

Through staged roasting and chemical modification, excessive or insufficient roasting is prevented, the activity recovery of the catalyst is significantly improved, and the performance of the catalyst after regeneration is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116060053B_ABST
    Figure CN116060053B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of catalyst regeneration, and discloses a regeneration method for a catalyst to be regenerated and an activity recovery method for a catalyst to be regenerated. The method comprises the following steps: (1) determining the peak result of a substance to be removed in the catalyst to be regenerated by a programmed temperature oxidation method; (2) performing programmed temperature roasting on the catalyst to be regenerated according to the peak result measured in step (1). The present invention provides a catalyst regeneration method, which roasts the catalyst to be regenerated in stages according to the peak temperature of the substance to be removed in the test result of the programmed temperature oxidation method, so as to promote the decomposition of each component in the catalyst to be regenerated, prevent over-roasting or under-roasting, and improve the activity recovery degree of the catalyst after regeneration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst regeneration, and in particular to a method for regenerating a catalyst to be regenerated and a method for restoring the activity of the catalyst to be regenerated. Background Art

[0002] Hydrogenation catalysts play an important role in the production of clean fuels and can remove impurities from crude oil. However, during use, the activity of hydrogenation catalysts gradually decreases, and the reaction temperature continues to rise until the upper limit of the operating temperature of the device. After the hydrogenation catalyst loses its activity, it needs to go through a regeneration step to restore its activity. Improving the activity of the catalyst can extend the operating cycle of the device. Therefore, the degree of activity recovery of the regenerated catalyst directly affects the life of the re-use. Therefore, it is necessary to develop deactivated catalyst regeneration technology to promote the reuse effect of hydrogenation catalysts.

[0003] There are many types of hydrogenation catalysts, and the deactivation and regeneration methods of different catalysts are not the same. Generally, the deactivated catalyst contains carbon deposits, and is generally regenerated by high-temperature calcination. This regeneration method has the advantage of universality, but the efficiency of this regeneration method is still somewhat insufficient. For deactivated catalysts with special pore structures, if high-temperature regeneration is directly performed, it is easy to cause problems such as incomplete calcination or over-calcination, and it is difficult to control the regeneration effect of the catalyst, and the optimal regeneration effect cannot be achieved.

[0004] In view of the deficiencies of the prior art, a method for regenerating a hydrogenation catalyst and a method for recovering its activity are provided to promote the effect of recovering the activity of the hydrogenation catalyst. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of incomplete or over-roasting in the high-temperature roasting regeneration method, and to provide a regeneration method for a catalyst to be regenerated and a method for recovering the activity of the catalyst to be regenerated. The method can prevent over-roasting or under-roasting and improve the degree of activity recovery of the regenerated catalyst.

[0006] In order to achieve the above object, the first aspect of the present invention provides a catalyst regeneration method, the method comprising the following steps:

[0007] (1) determining the peak results of the substance to be removed in the catalyst to be regenerated by a programmed temperature oxidation method;

[0008] (2) According to the peak result measured in step (1), the catalyst to be regenerated is subjected to programmed temperature calcination.

[0009] The second aspect of the present invention provides a method for restoring the activity of a catalyst to be regenerated, the method comprising: regenerating the catalyst to be regenerated according to the regeneration method described in the first aspect of the present invention to obtain a regenerated catalyst, then contacting the regenerated catalyst with an aqueous solution of an organic alcohol compound and / or a carboxylic acid compound, and then drying to obtain a catalyst with restored activity.

[0010] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0011] 1) A catalyst regeneration method provided by the present invention comprises performing segmented roasting on the catalyst to be regenerated according to the peak temperature of the substance to be removed in the test result of the programmed temperature oxidation method, which can promote the decomposition of each component in the catalyst to be regenerated, prevent over-roasting or under-roasting, and improve the activity recovery degree of the catalyst after regeneration;

[0012] 2) The present invention provides a method for recovering the activity of a catalyst to be regenerated, which can further recover the activity of the catalyst by adding an organic alcohol compound and / or a carboxylic acid compound to the regenerated catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a graph showing the test results of the programmed temperature oxidation method of the catalyst to be regenerated in Example 1. DETAILED DESCRIPTION

[0014] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0015] In the present invention, unless otherwise specified, the 2-6nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 6nm, the 2-4nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 4nm, the 4-6nm pores refer to pores with a pore diameter greater than or equal to 4nm and less than 6nm, and the 8-20nm pores refer to pores with a pore diameter greater than or equal to 8nm and less than 20nm.

[0016] A first aspect of the present invention provides a method for regenerating a catalyst to be regenerated, wherein the method comprises the following steps:

[0017] (1) determining the peak results of the substance to be removed in the catalyst to be regenerated by a programmed temperature oxidation method;

[0018] (2) According to the peak result measured in step (1), the catalyst to be regenerated is subjected to programmed temperature calcination.

[0019] In step (1):

[0020] In a preferred embodiment of the present invention, in the programmed temperature oxidation method, the carrier gas is selected from oxygen-containing gases, and the oxygen-containing gas is selected from air and / or oxygen, preferably air.

[0021] In a preferred embodiment of the present invention, in the programmed temperature oxidation method, the flow rate of the carrier gas is 30-200 mL / min, preferably 50-150 mL / min.

[0022] In one embodiment of the present invention, in the programmed temperature oxidation method, the temperature is increased from room temperature to 500-800° C. at a heating rate of 1-15° C. / min. The present invention does not specifically limit the room temperature, which may be 10-35° C.

[0023] In a preferred embodiment of the present invention, the present invention has no particular limitation on the specific schematic diagram of the catalyst to be regenerated, and it can be various catalysts to be regenerated in the conventional sense in the art, and its schematic diagram corresponds to the original catalyst (also referred to as fresh catalyst). In a preferred embodiment of the present invention, all non-fresh catalysts (i.e., catalysts after reaction) that can be regenerated by calcination can be regenerated by the regeneration method of the present invention.

[0024] In a preferred embodiment of the present invention, the original catalyst of the catalyst to be regenerated comprises at least one Group VIII metal element, at least one Group VIB metal element, optionally phosphorus pentoxide, and carrier alumina, and the pore size of the original catalyst of the catalyst to be regenerated presents a bimodal pore distribution in the range of 2-6nm and 8-20nm.

[0025] In the present invention, the pore size of the procatalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm, which means that the pore size distribution of the procatalyst has two peaks in the pore size range of 2-6nm and 8-20nm. Generally, the carrier also has a certain number of pore size distributions in the range of 2-6nm, but this part of the pores of the carrier does not have a peak, and no bimodal pores are formed.

[0026] In a preferred embodiment of the present invention, the Group VIII metal element includes but is not limited to at least one of Fe, Co, Ni, Ru, Pt and Pd, preferably Co and / or Ni.

[0027] In a preferred embodiment of the present invention, the VIB Group metal element includes but is not limited to at least one of Cr, Mo and W, preferably Mo and / or W.

[0028] In a preferred embodiment of the present invention, the water absorption rate of the alumina raw material used to prepare the original catalyst is greater than 0.9 mL / g, preferably 0.9-1.2 mL / g; preferably, the specific surface area of ​​the alumina raw material is greater than 260 m 2 / g, preferably 260-400m 2 / g; preferably, the average pore size of the alumina raw material is greater than 8nm, more preferably 8-14nm, and the pore distribution is a unimodal pore distribution; preferably, in the alumina raw material, the pore volume with a pore size distribution between 2-6nm accounts for no more than 10% of the total pore volume of the alumina raw material, more preferably no more than 8%, and more preferably 5-8%; in a particularly preferred case, in the alumina raw material, the pore volume with a pore size distribution between 2-4nm accounts for no more than 4% of the total volume of the alumina raw material, and more preferably no more than 2%.

[0029] In a preferred embodiment of the present invention, the specific surface area of ​​the procatalyst is 130-170 m 2 / g.

[0030] In a preferred embodiment of the present invention, the average pore size of the procatalyst is 6-18 nm, preferably 8-10 nm.

[0031] In a preferred embodiment of the present invention, the pore volume of the procatalyst is 0.2-0.4 cm 3 / g, preferably 0.25-0.4cm 3 / g.

[0032] In a preferred embodiment of the present invention, the volume of pores with a pore size distribution of 2-6 nm accounts for 8-15% of the total volume of the original catalyst, and more preferably 9-12%.

[0033] In the present invention, the determination of the specific surface area, pore volume, pore distribution and average pore size of the original catalyst refers to the determination after the catalyst is calcined at 400°C for 3 hours. The specific surface area, pore distribution, average pore size and pore volume of the original catalyst are determined by low temperature nitrogen adsorption method (BET) (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). Among them, the pore volume of 2-100nm is calculated according to the results of BET.

[0034] In a preferred embodiment of the present invention, the original catalyst composition is (Xi ai )·(Yi bi )·(Zi ci)·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-0.9nm, preferably 0.5-0.8nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup is the specific surface area of ​​the carrier. The specific surface area of ​​the carrier refers to the specific surface area of ​​the alumina raw material in the raw material for preparing the original catalyst. ρMoO3, ρWO3, ρNiO, ρCoO, ρP2O5 are 4.69 g / cm 3 , 7.16g / cm 3 、6.67g / cm 3 、6.45g / cm 3 and 2.39 g / cm 3 calculate.

[0035] In a preferred embodiment of the present invention, the molar ratio of Zi / Xi in the original catalyst is 0.05-0.3, and more preferably 0.08-0.2.

[0036] In a preferred embodiment of the present invention, the atomic concentration of the VIB group metal element in the original catalyst on the carrier surface is 5-13atom / nm 2 , preferably 5-11atom / nm 2 .

[0037] In the present invention, the atomic concentration of the VIB group metal element on the carrier surface refers to the average atomic concentration of the VIB group metal element on the carrier surface, which is obtained by measuring the metal loading and the specific surface area of ​​the carrier and then calculating. Specifically, it can be calculated as follows: atomic concentration = (ai / M Xi )×N A / (1×SA sup ), where N A is Avogadro's constant, ai is the mass relative to 1 gram of carrier Xi, M Xi is the molecular weight of Xi, SA sup is the specific surface area of ​​the carrier.

[0038] In a preferred embodiment of the present invention, the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the original catalyst is 0.05-0.35, preferably 0.1-0.3.

[0039] In a preferred embodiment of the present invention, the equivalent diameter of the procatalyst is 0.5-1.8 mm, more preferably 0.8-1.6 mm. In the present invention, there is no specific limitation on the shape of the procatalyst, and conventional catalyst shapes in the art are applicable to the present invention. Preferably, the catalyst is cylindrical, clover, four-leaf clover, butterfly, honeycomb or other irregular shapes, more preferably butterfly.

[0040] In a preferred embodiment of the present invention, the catalyst further comprises one or more organic alcohol compounds and / or carboxylic acid compounds, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds to the Group VIII metal elements is 1-6, preferably 2-5.

[0041] The organic alcohol compound can be at least one of a monohydric alcohol, a dihydric alcohol and a polyhydric alcohol. In a preferred embodiment, the organic alcohol compound is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane, preferably at least one of glycerol, propanol and ethylene glycol.

[0042] In a preferred embodiment, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, preferably at least one of formic acid, citric acid and acetic acid.

[0043] In a particularly preferred case, the procatalyst also comprises one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol, trimethylolethane and / or formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid, tartaric acid.

[0044] In a preferred embodiment of the present invention, the substance to be removed includes at least one of carbon deposits, sulfides, and nitrogen-containing organic matter.

[0045] In a preferred embodiment of the present invention, the components to be removed include carbon deposits and sulfides.

[0046] In a preferred embodiment of the present invention, the carbon content in the catalyst to be regenerated is 1-10 wt%, and the sulfur content is 1-20 wt%, wherein the carbon and sulfur contents are calculated by element weight.

[0047] In step (2):

[0048] In a preferred embodiment of the present invention, the number of peaks n and the peak temperature T of each peak are determined according to the peak results. i ; Wherein, i is an integer from 1 to n.

[0049] In the present invention, when a programmed temperature oxidation test is performed on the catalyst to be regenerated, if the difference in peak temperatures between two adjacent peaks is within 10° C., they can be regarded as one peak, and the peak temperature is the average value of the peak temperatures of the two peaks.

[0050] In a preferred embodiment of the present invention, in the calcination temperature program of the programmed temperature calcination, the temperature program in the calcination temperature program is divided into n sections according to the peak result, and the final temperature in each section of the calcination temperature program corresponds to T i .

[0051] In a preferred embodiment of the present invention, the heating rate in each calcination heating program is independently selected from 1-20°C / min, preferably 2-15°C / min.

[0052] In a preferred embodiment of the present invention, the constant temperature time of the final temperature in each stage of the calcination temperature rise program is independently selected from 1-10 hours, preferably 3-6 hours.

[0053] In a preferred embodiment of the present invention, the heating rate in the first stage of the roasting temperature rising program is not less than the heating rate in the second stage of the roasting temperature rising program to the Nth stage of the roasting temperature rising program.

[0054] In a preferred embodiment of the present invention, the heating rate decreases successively from the first stage to the Nth stage of the roasting heating program. Further preferably, the heating rate decreases successively by 1-10°C / min, preferably by 2-7°C / min, between adjacent roasting heating program stages.

[0055] Among them, in the present invention, by controlling the heating rate of each stage of roasting, the regeneration effect can be further improved and the activity recovery degree of the regenerated catalyst can be increased.

[0056] In a preferred embodiment of the present invention, in the roasting temperature rising program, the roasting temperature rising program further includes an n+1 stage, in which the temperature is raised to T n +10℃ to T n +50℃, preferably heated to T n +15℃ to T n Calcination was carried out at +30°C.

[0057] In a preferred embodiment of the present invention, in the n+1th stage of the calcination temperature increase program, the heating rate is 1-10° C. / min, preferably 1-5° C. / min.

[0058] In a preferred embodiment of the present invention, in the n+1th stage of the calcination temperature rise program, the constant temperature time is 1-5 hours, preferably 2-4 hours.

[0059] Among them, the inventor of the present invention has found through research that in T n After constant temperature calcination at a certain temperature, the regeneration activity of the regenerated catalyst can be further improved by continuing to increase the temperature for a period of time.

[0060] In a preferred embodiment of the present invention, the programmed temperature calcination is carried out in an air atmosphere.

[0061] A second aspect of the present invention provides a method for recovering the activity of a catalyst to be regenerated, the method comprising:

[0062] The catalyst to be regenerated is regenerated according to the regeneration method described in the first aspect of the present invention to obtain a regenerated catalyst, and then the regenerated catalyst is contacted with an aqueous solution of an organic alcohol compound and / or a carboxylic acid compound, and then dried to obtain a catalyst with restored activity.

[0063] In a preferred embodiment of the present invention, the original catalyst of the catalyst to be regenerated contains an organic alcohol compound and / or a carboxylic acid compound.

[0064] In a preferred embodiment of the present invention, the organic alcohol compound is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane, preferably at least one of glycerol, propanol and ethylene glycol.

[0065] In a preferred embodiment of the present invention, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, preferably at least one of formic acid, citric acid and acetic acid.

[0066] In a preferred embodiment of the present invention, the organic alcohol compound and / or carboxylic acid compound are of the same type as the organic alcohol compound and / or carboxylic acid compound in the original catalyst.

[0067] In a preferred embodiment of the present invention, the amount of the organic alcohol compound and / or carboxylic acid compound added is 0.5-2 times, preferably 0.75-1.5 times, the amount of the organic alcohol compound and / or carboxylic acid compound in the original catalyst.

[0068] The present invention will be described in detail below through examples.

[0069] The amount of material added during the preparation of the original catalyst is determined according to the specific exemplary description given in the text of the present invention.

[0070] Exemplary description: (1) According to the atomic concentration of the VIB group metal element and the specific surface area of ​​the carrier (alumina), the amount of the VIB group metal precursor per gram of the carrier is determined; (2) According to the atomic ratio of the VIII group metal element to the total amount of the VIII group metal element and the VIB group metal element, the amount of the VIII group metal precursor per gram of the carrier is determined; (3) According to (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA supThe content of P2O5 is calculated based on the value of , and then the amount of phosphorus-containing compound in each gram of carrier is determined; (4) the amount of organic alcohol compound and / or carboxylic acid compound is calculated based on the molar ratio of organic alcohol compound and / or carboxylic acid compound to Group VIII metal element; (5) according to the feed amounts of Group VIB metal precursor, Group VIII metal precursor, phosphorus-containing compound and organic alcohol compound and / or carboxylic acid compound, alumina is impregnated with impregnation solution by pore saturation impregnation method, and then dried. Specifically, the phosphorus-containing compound is first dissolved in water, and then an organic alcohol compound and / or a carboxylic acid compound, a Group VIB metal precursor and a Group VIII metal precursor are added, and the mixture is stirred under heating until it is completely dissolved, and the temperature is kept constant to obtain an impregnation solution; (6) the water absorption rate of the carrier is measured, and the liquid absorption rate of the carrier is calculated according to the formula of carrier water absorption rate-0.1; (7) according to the liquid absorption rate of the carrier, the impregnation solution is adjusted to a corresponding volume (carrier liquid absorption rate×carrier mass), and the impregnation solution and the corresponding mass of the carrier are evenly mixed and allowed to stand, and then dried to prepare a catalyst.

[0071] In the following examples, the composition of the catalyst is calculated based on the feed amount. The specific surface area of ​​2-100 nm in the catalyst and the carrier, the pore distribution, the pore diameter, and the pore volume are determined by low temperature nitrogen adsorption (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The sulfur mass fraction in the product is analyzed using a sulfur nitrogen analyzer (produced by Thermo Fisher Scientific, model TN / TS3000), and the content of aromatics is analyzed by near infrared spectroscopy.

[0072] The hydrodesulfurization performance of the catalyst was measured on a 20mL high-pressure microreactor, and the oxidized catalyst was directly converted into the sulfurized catalyst using a programmed temperature sulfurization method. The sulfurization conditions were: the sulfurization pressure was 6.4MPa, the sulfurized oil was kerosene containing 2% by weight of CS2, and the volume space velocity was 2 hours. -1 , the hydrogen-to-oil volume ratio is 300v / v, first keep the temperature at 230℃ / h for 6h, then heat it up to 360℃ for sulfidation for 8h, and the heating rate of each stage is 10℃ / h. After sulfidation, switch the reaction raw materials for hydrodesulfurization activity test. The reaction raw materials have a sulfur content of 10890ppm and an aromatic content of 39.0wt% of high aromatic distillate oil. The test conditions are: pressure of 6.4MPa, volume space velocity of 1.5h -1 , the hydrogen-oil volume ratio is 300 v / v, and the reaction temperature is 340°C.

[0073] The programmed temperature oxidation method was carried out on a thermogravimetric mass spectrometer (NETZSCH STA 409PC / PG) instrument. The specific operating conditions were: air was used as the carrier gas, the flow rate of the carrier gas was 50 mL / min, the sample was heated from room temperature to 600°C at a heating rate of 10°C / min for a programmed temperature oxidation test, and a mass spectrometer was used to monitor the gas outlet of the instrument to obtain a curve of the sample decomposition product changing with temperature.

[0074] The activity of the catalyst is defined as the hydrodesulfurization reaction rate constant (k HDS ), the reaction order is calculated according to 1.2, and the calculation formula is: k HDS =1 / (n-1)×(s p (1-n) -s f (1-n) )×LHSV, where n is the reaction rate constant, S p is the sulfur content in the product, S f is the sulfur content in the raw materials.

[0075] The catalyst activity recovery degree is defined as: the ratio of the hydrodesulfurization reaction rate constant of the regenerated catalyst to the hydrodesulfurization reaction rate constant of the fresh catalyst×100%.

[0076] Example 1

[0077] (1) Preparation of procatalyst

[0078] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0079] MoO3, basic nickel carbonate and glycerol were added to a phosphoric acid aqueous solution, heated and stirred at 85°C for 2 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0080] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0081] The atomic concentration of Mo in the catalyst is 7atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.29, P2O5 / MoO3 molar ratio is 0.13, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi) / SA sup is 0.5 nm, and the molar ratio of glycerol to Ni is 2.

[0082] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 165m 2 / g, pore volume 0.38cm 3 / g, the average pore diameter is 9.2nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 9.2% of the total pore volume.

[0083] (2) Catalyst testing

[0084] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a catalyst to be regenerated. The substances to be removed from the catalyst to be regenerated include carbon deposits and sulfides, and the carbon and sulfur contents in the catalyst to be regenerated are 6.8wt% and 10.5wt%, respectively.

[0085] (3) Regeneration of the catalyst to be regenerated

[0086] The catalyst to be regenerated was subjected to a programmed temperature oxidation test to determine that the number of peaks of the substance to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 340°C, the peak temperature of the second peak was 440°C, and the third temperature was 450°C.

[0087] The catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, with the temperature being increased from room temperature to 340°C at a heating rate of 10°C / min, and kept at the constant temperature for 5 hours, and then increased to 445°C at a heating rate of 5°C / min, and kept at the constant temperature for 5 hours, and finally increased to 470°C at a heating rate of 2°C / min and kept at the constant temperature for 4 hours to obtain a regenerated catalyst;

[0088] The regenerated catalyst and the glycerol aqueous solution were mixed evenly by an equal volume impregnation method, and dried at 130° C. for 3 hours to obtain a catalyst with restored activity, wherein the amount of glycerol used was 1.5 times the glycerol content in the original catalyst.

[0089] After the catalyst with restored activity was retested for hydrodesulfurization performance, the degree of activity recovery was 96%.

[0090] Example 2

[0091] (1) Preparation of procatalyst

[0092] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0093] MoO3, basic nickel carbonate and glycerol were added to the phosphoric acid aqueous solution, heated and stirred at 90°C for 3 hours until completely dissolved and kept at constant temperature for 3 hours to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0094] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0095] The atomic concentration of Mo in the catalyst is 11atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.1, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.72 nm, and the molar ratio of glycerol to Ni is 5.

[0096] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 151m 2 / g, pore volume 0.32cm 3 / g, the average pore diameter is 8.5nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 9% of the total pore volume.

[0097] (2) Catalyst testing

[0098] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a catalyst to be regenerated. The substances to be removed from the catalyst to be regenerated include carbon deposits and sulfides, and the carbon and sulfur contents in the catalyst to be regenerated are 7.6wt% and 12.3wt%, respectively.

[0099] (3) Regeneration of the catalyst to be regenerated

[0100] The catalyst to be regenerated was subjected to a programmed temperature oxidation test to determine that the number of peaks of the substance to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 340°C, and the peak temperature of the second peak was 430°C.

[0101] The catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, with the temperature being increased from room temperature to 340°C at a heating rate of 8°C / min, and kept at the constant temperature for 5 hours, and then increased to 430°C at a heating rate of 3°C / min, and kept at the constant temperature for 5 hours, and finally increased to 460°C at a heating rate of 1.5°C / min and kept at the constant temperature for 4 hours to obtain a regenerated catalyst;

[0102] The regenerated catalyst and the glycerol aqueous solution were mixed evenly by an equal volume impregnation method, and dried at 130° C. for 3 hours to obtain a catalyst with restored activity, wherein the amount of glycerol used was 0.8 times the glycerol content in the original catalyst.

[0103] After the catalyst with restored activity was retested for hydrodesulfurization performance, the degree of activity recovery was 94%.

[0104] Example 3

[0105] (1) Preparation of procatalyst

[0106] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0107] MoO3, basic nickel carbonate and glycerol were added to a phosphoric acid aqueous solution, heated and stirred at 90°C for 3 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 2 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0108] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0109] The atomic concentration of Mo in the catalyst is 8atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.623nm, and the molar ratio of glycerol to Ni is 3.

[0110] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 164m 2 / g, pore volume 0.35cm 3 / g, the average pore size is 8.5nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for a proportion of the total pore volume.

[0111] (2) Catalyst testing

[0112] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a catalyst to be regenerated. The substances to be removed from the catalyst to be regenerated include carbon deposits and sulfides, and the carbon and sulfur contents in the catalyst to be regenerated are 6.5wt% and 10.2wt%, respectively.

[0113] (3) Regeneration of the catalyst to be regenerated

[0114] The catalyst to be regenerated was subjected to a programmed temperature oxidation test to determine that the number of peaks of the substance to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 320°C, and the peak temperature of the second peak was 440°C.

[0115] The catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, with the temperature being increased from room temperature to 320°C at a heating rate of 10°C / min, and kept at the constant temperature for 5 hours, and then increased to 440°C at a heating rate of 3°C / min, and kept at the constant temperature for 5 hours, and finally increased to 470°C at a heating rate of 1.5°C / min and kept at the constant temperature for 4 hours to obtain a regenerated catalyst;

[0116] The regenerated catalyst was mixed evenly with a glycerol aqueous solution by an equal volume impregnation method, and dried at 130° C. for 3 hours to obtain a catalyst with restored activity, wherein the amount of glycerol used was 1.2 times the glycerol content in the original catalyst.

[0117] After the catalyst with restored activity was retested for hydrodesulfurization performance, the degree of activity recovery was 96%.

[0118] Example 4

[0119] (1) Preparation of procatalyst

[0120] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0121] Ammonium metatungstate, basic nickel carbonate and citric acid were added to the phosphoric acid aqueous solution respectively, heated and stirred at 90°C for 2 hours until completely dissolved and kept at constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 2 hours, and dried at 130°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0122] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0123] The atomic concentration of W in the catalyst is 5atom / nm 2 , Ni / (Ni+W) atomic ratio is 0.3, P2O5 / WO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.407 nm, and the molar ratio of citric acid to Ni is 2.

[0124] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 162m 2 / g, pore volume 0.39cm 3 / g, the average pore diameter is 9.6nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 10.5% of the total pore volume.

[0125] (2) Catalyst testing

[0126] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a catalyst to be regenerated. The substances to be removed from the catalyst to be regenerated include carbon deposits and sulfides, and the carbon and sulfur contents in the catalyst to be regenerated are 6.4wt% and 7.8wt%, respectively.

[0127] (3) Regeneration of the catalyst to be regenerated

[0128] The catalyst to be regenerated was subjected to a programmed temperature oxidation test to determine that the number of peaks of the substance to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 300°C, and the peak temperature of the second peak was 455°C.

[0129] The catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, with the temperature being increased from room temperature to 300°C at a heating rate of 10°C / min, and kept at the constant temperature for 5 hours, and then increased to 455°C at a heating rate of 3°C / min, and kept at the constant temperature for 5 hours, and finally increased to 470°C at a heating rate of 2°C / min and kept at the constant temperature for 4 hours to obtain a regenerated catalyst;

[0130] The regenerated catalyst and the citric acid aqueous solution were mixed evenly by an equal volume impregnation method, and dried at 130° C. for 3 hours to obtain a catalyst with restored activity, wherein the amount of citric acid used was 1.5 times the citric acid content in the original catalyst.

[0131] After the catalyst with restored activity was retested for hydrodesulfurization performance, the degree of activity recovery was 97%.

[0132] Example 5

[0133] (1) Preparation of procatalyst

[0134] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of ​​270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0135] MoO3, basic nickel carbonate and citric acid were added to a phosphoric acid aqueous solution, heated and stirred at 85°C for 3 hours until completely dissolved and kept at a constant temperature for 2 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0136] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0137] The atomic concentration of Mo in the catalyst is 9atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.12, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.62 nm, and the molar ratio of citric acid to Ni is 2.

[0138] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 154m 2 / g, pore volume 0.36cm 3 / g, the average pore diameter is 9.4nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 9.8% of the total pore volume.

[0139] (2) Catalyst testing

[0140] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a catalyst to be regenerated. The substances to be removed from the catalyst to be regenerated include carbon deposits and sulfides, and the carbon and sulfur contents in the catalyst to be regenerated are 7.4wt% and 11.1wt%, respectively.

[0141] (3) Regeneration of the catalyst to be regenerated

[0142] The catalyst to be regenerated was subjected to a programmed temperature oxidation test to determine that the number of peaks of the substance to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 340°C, and the peak temperature of the second peak was 420°C.

[0143] The catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, with the temperature being increased from room temperature to 340°C at a heating rate of 6°C / min, and kept at the constant temperature for 5 hours, and then increased to 420°C at a heating rate of 3°C / min, and kept at the constant temperature for 5 hours, and finally increased to 460°C at a heating rate of 1°C / min and kept at the constant temperature for 4 hours to obtain a regenerated catalyst;

[0144] The regenerated catalyst and the citric acid aqueous solution were mixed evenly by an equal volume impregnation method, and dried at 150° C. for 3 hours to obtain a catalyst with restored activity, wherein the amount of citric acid used was 1 times the citric acid content in the original catalyst.

[0145] After the catalyst with restored activity was retested for hydrodesulfurization performance, the degree of activity recovery was 94%.

[0146] Example 6

[0147] (1) Preparation of procatalyst

[0148] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of ​​270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0149] MoO3, basic nickel carbonate and citric acid were added to a phosphoric acid aqueous solution, heated and stirred at 95°C for 3 hours until completely dissolved and kept at a constant temperature for 2 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0150] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0151] The atomic concentration of Mo in the catalyst is 10atom / nm2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.27, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.85 nm, and the molar ratio of citric acid to Ni is 2.

[0152] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 135m 2 / g, pore volume 0.27cm 3 / g, the average pore diameter is 8.0nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 12.5% ​​of the total pore volume.

[0153] (2) Catalyst testing

[0154] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a catalyst to be regenerated. The substances to be removed from the catalyst to be regenerated include carbon deposits and sulfides, and the carbon and sulfur contents in the catalyst to be regenerated are 6.2wt% and 11.8wt%, respectively.

[0155] (3) Regeneration of the catalyst to be regenerated

[0156] The catalyst to be regenerated was subjected to a programmed temperature oxidation test to determine that the number of peaks of the substance to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 330°C, and the peak temperature of the second peak was 425°C.

[0157] The catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, with the temperature being increased from room temperature to 330°C at a heating rate of 6°C / min, and kept at the constant temperature for 5 hours, and then increased to 425°C at a heating rate of 3°C / min, and kept at the constant temperature for 5 hours, and finally increased to 465°C at a heating rate of 1.5°C / min and kept at the constant temperature for 4 hours to obtain a regenerated catalyst;

[0158] The regenerated catalyst and the citric acid aqueous solution were mixed evenly by an equal volume impregnation method, and dried at 150° C. for 3 hours to obtain a catalyst with restored activity, wherein the amount of citric acid used was 1 times the citric acid content in the original catalyst.

[0159] After the catalyst with restored activity was retested for hydrodesulfurization performance, the degree of activity recovery was 94%.

[0160] Example 7

[0161] The method is the same as Example 1, except that the last high-temperature calcination is not performed. Specifically, in step (3) of regenerating the catalyst to be regenerated, the catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere. The temperature is increased from room temperature to 340°C at a heating rate of 5°C / h, and the temperature is maintained for 5 hours. The temperature is then increased to 445°C at a heating rate of 2°C / h, and the temperature is maintained for 5 hours to obtain a regenerated catalyst.

[0162] After the activity test, the activity recovery degree of the catalyst with restored activity was 91.5%.

[0163] Example 8

[0164] The method is the same as Example 1, except that, in step (3) of regenerating the catalyst to be regenerated, the catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, with the temperature being increased from room temperature to 340°C at a heating rate of 5°C / min, and kept at the constant temperature for 5 hours, then increased to 445°C at a heating rate of 5°C / min, and kept at the constant temperature for 5 hours, and finally increased to 470°C at a heating rate of 5°C / min and kept at the constant temperature for 4 hours to obtain a regenerated catalyst.

[0165] After the activity test, the activity recovery degree of the catalyst with restored activity was 94.5%.

[0166] Example 9

[0167] The method is the same as Example 1, except that, in step (3) of regenerating the catalyst to be regenerated, the catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, with the temperature being increased from room temperature to 340°C at a heating rate of 2°C / min and kept at the constant temperature for 5 hours, then increased to 445°C at a heating rate of 5°C / min and kept at the constant temperature for 5 hours, and finally increased to 470°C at a heating rate of 10°C / min and kept at the constant temperature for 4 hours to obtain a regenerated catalyst.

[0168] After the catalyst with restored activity was retested for hydrodesulfurization performance, the degree of activity recovery was 88.7%.

[0169] Comparative Example 1

[0170] The same as Example 1, except that, in step (3) of regenerating the catalyst to be regenerated, the catalyst to be regenerated is directly placed in a muffle furnace, and the temperature is increased from room temperature to 470°C at a heating rate of 5°C / min in an air atmosphere, and the temperature is maintained at a constant level for 14 hours.

[0171] After the catalyst with restored activity was retested for hydrodesulfurization performance, the degree of activity recovery was 86.2%.

[0172] It can be seen from the examples and comparative examples that the present invention has good inventive effects, the catalyst regeneration method and the prepared regenerated catalyst have high activity and stability, and have good industrial application prospects.

[0173] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for regenerating a catalyst to be regenerated, It is characterized in that The method comprises the following steps: (1) Determining the peak results of the substance to be removed in the catalyst to be regenerated by a programmed temperature oxidation method; In step (1), according to the peak results, the number of peaks n and the peak temperature T of each peak are determined. i ; Wherein, i is an integer from 1 to n; (2) According to the peak results measured in step (1), the catalyst to be regenerated is subjected to programmed temperature calcination; In step (2), in the calcination temperature program of the programmed temperature calcination, the calcination temperature program is divided into n sections according to the peak result, and the final temperature in each section of the calcination temperature program corresponds to T i ; The heating rate in each calcination heating program is independently selected from 1-20°C / min; The original catalyst of the catalyst to be regenerated comprises at least one metal element of Group VIII, at least one metal element of Group VIB, optional phosphorus pentoxide, and carrier alumina, and the pore size is in the range of 2-6nm and 8-20nm, presenting a bimodal pore distribution.

2. The regeneration method according to claim 1, in, The heating rate in each calcination heating program is independently selected from 2-15°C / min.

3. The regeneration method according to claim 1 or 2, in, The final temperature constant temperature time in each roasting temperature rising program is independently selected from 1-10h.

4. The regeneration method according to claim 3, in, The constant temperature time of the final temperature in each roasting temperature rising program is independently selected from 3-6h.

5. The regeneration method according to claim 1 or 2, in, The heating rate in the first stage of the roasting temperature rising program is not less than the heating rate in the second stage of the roasting temperature rising program to the Nth stage of the roasting temperature rising program.

6. The regeneration method according to claim 5, in, From the first stage of the roasting temperature rise program to the Nth stage of the roasting temperature rise program, the heating rate decreases successively.

7. The regeneration method according to claim 6, in, Between adjacent roasting temperature rising program sections, the heating rate decreases by 1-10℃ / min.

8. The regeneration method according to claim 7, in, Between adjacent roasting temperature rising program sections, the heating rate decreases by 2-7℃ / min.

9. The regeneration method according to claim 1 or 2, in, In step (2), in the roasting temperature rising program, the roasting temperature rising program also includes an n+1 stage, in which the temperature is raised to T n +10℃ to T n Calcination was carried out at +50°C.

10. The regeneration method according to claim 9, in, In step (2), in the n+1th stage of the calcination temperature increase program, the heating rate is 1-10°C / min.

11. The regeneration method according to claim 10, in, In step (2), in the n+1th stage of the calcination temperature increase program, the heating rate is 1-5°C / min.

12. The regeneration method according to claim 9, in, In step (2), in the n+1th stage of the calcination temperature rise program, the constant temperature time is 1-5 hours.

13. The regeneration method according to claim 12, in, In step (2), in the n+1th stage of the calcination temperature rise program, the constant temperature time is 2-4 hours.

14. The regeneration method according to claim 1 or 2, in, The substance to be removed includes at least one of carbon deposits, sulfides, and nitrogen-containing organic matter.

15. The regeneration method according to claim 14, in, The catalyst to be regenerated has a carbon content of 1-10 wt % and a sulfur content of 1-20 wt %.

16. The regeneration method according to claim 1 or 2, in, The original catalyst composition of the catalyst to be regenerated is (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, where Xi is the metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is the metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P 2 O 5 , ci is relative to 1 gram of carrier P 2 O 5 The mass of Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-0.9nm, ρ Xi , Yi , Zi are Group VIB metal oxides, Group VIII metal oxides and P 2 O 5 The density of SA sup is the specific surface area of ​​the carrier.

17. The regeneration method according to claim 16, in, The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.5-0.8nm.

18. The regeneration method according to claim 16, in, The molar ratio of Zi / Xi in the original catalyst is 0.05-0.

3.

19. The regeneration method according to claim 18, in, The molar ratio of Zi / Xi in the original catalyst is 0.08-0.

2.

20. The regeneration method according to claim 1 or 2, in, The atomic concentration of the VIB group metal element in the procatalyst on the carrier surface is 5-13atom / nm 2 .

21. The regeneration method according to claim 20, in, The atomic concentration of the VIB group metal element in the procatalyst on the carrier surface is 5-11atom / nm 2 .

22. The regeneration method according to claim 1 or 2, in, The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the procatalyst is 0.05-0.

35.

23. The regeneration method according to claim 22, in, The atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the procatalyst is 0.1-0.

3.

24. The regeneration method according to claim 22, in, The procatalyst further comprises one or more organic alcohol compounds and / or carboxylic acid compounds, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds to the metal element of Group VIII is 1-6.

25. The regeneration method according to claim 24, in, The molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is 2-5.

26. A method for restoring the activity of a catalyst to be regenerated, It is characterized in that The method includes: The catalyst to be regenerated is regenerated according to the regeneration method according to any one of claims 1 to 25 to obtain a regenerated catalyst, and then the regenerated catalyst is contacted with an aqueous solution of an organic alcohol compound and / or a carboxylic acid compound, and then dried to obtain a catalyst with restored activity.

27. The method for restoring the activity of a catalyst to be regenerated according to claim 26, in, The original catalyst of the catalyst to be regenerated contains organic alcohol compounds and / or carboxylic acid compounds.

28. The activity recovery method according to claim 26 or 27, in, The organic alcohol compound is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane.

29. The activity recovery method according to claim 28, in, The organic alcohol compound is selected from glycerol and / or propanol.

30. The activity recovery method according to claim 26 or 27, in, The carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid.

31. The activity recovery method according to claim 30, in, The carboxylic acid compound is selected from at least one of formic acid, citric acid and acetic acid.

32. The activity recovery method according to claim 26 or 27, in, The organic alcohol compound and / or carboxylic acid compound are of the same type as the organic alcohol compound and / or carboxylic acid compound in the original catalyst.

33. The activity recovery method according to claim 32, in, The amount of the organic alcohol compound and / or carboxylic acid compound added is 0.5-2 times the content of the organic alcohol compound and / or carboxylic acid compound in the original catalyst.

34. The activity recovery method according to claim 32, in, The amount of the organic alcohol compound and / or carboxylic acid compound added is 0.75-1.5 times the content of the organic alcohol compound and / or carboxylic acid compound in the original catalyst.

Citation Information

Patent Citations

  • Nickel containing mixed metal-oxide / carbon bulk hydroprocessing catalysts and their application

    CA3013302A1

  • Reformed pre-hydrogenation catalyst and preparation method thereof

    CN103143367A

  • Hydrodeoxygenation method of bio-oil as well as catalyst and preparation method used thereby

    CN105903475A

  • Method for regenerating a catalyst which is spent and regenerated by a hydrodesulfurization process of gasolines

    CN113438971A

  • Hydrorefining catalyst, preparation method therefor and use thereof

    WO2019196836A1