A silicon capture catalyst and preparation method thereof

By loading a molecular sieve and a silicon-capturing catalyst with active components on an alumina carrier, the problems of high silicon-capturing agent cost and poor silicon-capturing ability in the existing technology are solved, achieving efficient silicon capturing and hydrogenation activity, and prolonging the device life. operating cycle.

CN116060081BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111278929.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-31
Publication Date
2024-10-01
Estimated Expiration
2041-10-31

AI Technical Summary

Technical Problem

Existing silicon-capturing catalysts have problems such as high preparation costs and poor silicon-capturing ability during the coking process, which leads to silicon poisoning of the main catalyst and affects the operation cycle of the device.

Method used

Alumina is used as a carrier silicon capture catalyst to load molecular sieves and active components, including Group VIB metal oxides and Group VIII metal oxides. The metal ratio and molecular sieve loading method are optimized through CO-FTIR analysis to increase the pore volume of the catalyst. and specific surface area to enhance its silicon capture and hydrogenation activities.

Benefits of technology

It achieves efficient silicon capture and reduces catalyst costs, improves hydrogenation activity and silicon capture capacity, and extends the device operation cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 917721DEST_PATH_IMAGE002
    Figure 917721DEST_PATH_IMAGE002
  • Figure DEST_PATH_IMAGE001
    Figure DEST_PATH_IMAGE001
Patent Text Reader

Abstract

The present invention provides a silicon-capturing catalyst and a preparation method thereof, wherein alumina is used as a carrier, and a molecular sieve and an active component are loaded thereon, wherein the active component is an oxide of a metal of Group VIB and an oxide of a metal of Group VIII, and the molecular sieve is loaded on the outer surface of the catalyst. The catalyst uses alumina powder and a sulfide powder of a metal of Group VIB as raw materials, obtains a precursor, impregnates a metal salt of Group VIII, and then hydrothermally treats the molecular sieve precursor, dries, and roasts to obtain the catalyst. The catalyst of the present invention allows the molecular sieve to be loaded on the outer surface of the catalyst instead of being kneaded with the carrier, which is beneficial to increasing the contact surface between the molecular sieve and the active metal, increasing the probability of the molecular sieve contacting with the cyclosiloxane compound, and improving the silicon-capturing ability of the catalyst; the utilization rate of the molecular sieve is increased, thereby reducing the amount of the molecular sieve used and reducing the cost of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil hydrogenation, and in particular to a silicon-capturing catalyst and a preparation method thereof. Background Art

[0002] At present, there are still a large number of delayed coking units in my country that process heavy and inferior oils. Defoamers are used in the process, which results in a certain amount of silicon in products such as coking dry gas, coking naphtha, and coking diesel. Silicon poisons the catalysts used in the subsequent treatment of coking products, leading to permanent deactivation of the catalysts. Therefore, the hydroprocessing processes of coking dry gas, coking naphtha, and coking diesel all require the loading of silicon-capturing catalysts, which require the silicon-capturing catalysts to have not only strong silicon-capturing capabilities but also certain hydrogenation activity. Studies have found that the silicon types in coking products are mainly cyclosiloxane compounds. To capture silicon on the silicon-capturing catalyst, the silicon-oxygen ring of the cyclosiloxane must be opened, which requires the silicon-capturing catalyst to have a higher acidity.

[0003] CN201911020761.2 discloses a silicon trap and a preparation method thereof. The silicon trap of the invention comprises a carrier and a hydrogenation active component, wherein the hydrogenation active component is a VIB group metal sulfide, a VIB group metal oxide and a VIII group metal oxide. Based on the total weight of the silicon trap, the VIB group metal sulfide is 0.3wt%-18.3wt%, the VIB group metal oxide is 0.1wt%-5.0wt%, and the VIII group metal oxide is 0.2wt%-12.0wt%. The preparation method of the silicon trap of the invention comprises the following contents: (1) impregnating a catalyst carrier with an impregnation solution containing a VIB group metal, then drying the catalyst carrier, and then subjecting the dried catalyst carrier to a sulfurization treatment; (2) impregnating the catalyst carrier with an impregnation solution containing a VIB group metal and a VIII group metal into the catalyst carrier after sulfurization in step (1), and then drying and calcining the catalyst carrier in an inert atmosphere to obtain the silicon trap.

[0004] CN200910188090.0 discloses a coking naphtha silicon scavenger and its application. The coking naphtha silicon scavenger uses alumina as a carrier, silicon dioxide as an auxiliary agent, and W, Mo and Ni as hydrogenation components. The pore volume of the coking naphtha silicon scavenger is 0.5-0.70 mL / g, and the specific surface area is 250-500 m 2 / g, the content of hydrogenated components is 1% to 20% calculated as oxide, and the acid content is 0.3 to 0.5 mmol / g.

[0005] Although many researchers have improved the silicon-capturing capacity of silicon scavengers through various methods and means, there are still problems such as high preparation cost and poor silicon-capturing capacity, which affects the operation cycle of the device and causes silicon poisoning of the main catalyst. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention discloses a silicon-capturing catalyst and a preparation method thereof. The catalyst not only has a high silicon-capturing capacity, but also has a certain hydrogenation saturation capacity.

[0007] In the context of this specification, CO-FTIR (carbon monoxide in-situ infrared analysis) is used to analyze the content of Group VIII metal oxides on Group VIB metal oxide wafers. The measurement conditions of the CO-FTIR include: after the catalyst is ground, it is pressed into a Φ13mm self-supporting sheet and placed on the in-situ cell sample holder. It is treated with 3.0% H2S at 320°C for 3h, then cooled to room temperature in an H2S atmosphere, and then vacuumed to 300°C for purification for 2h, and CO adsorption is performed under liquid nitrogen to reduce the temperature. A small amount of CO gas is introduced into the in-situ cell, and after adsorption equilibrium for 30 min, it is desorbed to 10 -4 Pa. The infrared spectra before and after the adsorption of CO were collected, and the difference between the two spectra was the infrared spectrum result of the catalyst adsorbing CO. The experiment used Nicolet 6700 Fourier transform infrared spectrometer, with 32 scans and a resolution of 4 cm -1 , 4000~650cm -1 Measurement, detector is MCT / A.

[0008] In order to achieve the above technical objectives, the technical solution of the present invention is as follows:

[0009] The technical purpose of the first aspect of the present invention is to provide a silicon capture catalyst, which uses aluminum oxide as a carrier, on which molecular sieves and active components are loaded, wherein the active components are oxides of Group VIB metals and oxides of Group VIII metals. Based on the total weight of the catalyst, the molecular sieve accounts for 1-12wt%, preferably 1.5-8wt%, and more preferably 2-6wt%; the Group VIB metal is calculated as oxide at 2-15%, preferably 5-10%, and the Group VIII metal is calculated as oxide at 2-10%, preferably 4-8%; the content of the Group VIII metal oxide on the Group VIB metal oxide wafer accounts for 60-100% of the Group VIII metal oxide; and the molecular sieve is loaded on the outer surface of the catalyst.

[0010] Furthermore, the pore volume of the silicon capture catalyst is 0.5-1.0 mL / g, preferably 0.7-1.0 mL / g; the specific surface area is 250-500 m 2 / g, preferably 350-500m 2 / g; the acid content of B is 0.05-0.3mmol / g, preferably 0.08-0.2mmol / g.

[0011] Furthermore, when the silicon-trapping catalyst is analyzed by CO-FTIR, the molar ratio of the Group VIB metal-Group VIII metal-S phase to the Group VIII metal is 60-100%, preferably 65%-90%, more preferably 70%-90%, and most preferably 80%-90%.

[0012] Furthermore, the molecular sieve is at least one selected from Y-type molecular sieve, ZSM-5 molecular sieve, β-type molecular sieve and MCM-41 molecular sieve.

[0013] Furthermore, the molecular sieve loaded on the outer surface of the catalyst is loaded on a VIB group metal oxide, and / or loaded on a VIII group metal oxide, and / or loaded on alumina.

[0014] Furthermore, the Group VIB metal oxide is molybdenum trioxide and / or tungsten trioxide, and the Group VIII metal oxide is nickel oxide and / or cobalt oxide.

[0015] The technical purpose of the second aspect of the present invention is to provide a method for preparing the above-mentioned silicon capture catalyst, comprising the following steps:

[0016] (1) Alumina powder, sulfide powder of Group VIB metal, peptizing agent and extrusion aid are mixed, extruded into strips, and dried and calcined to obtain catalyst precursor A;

[0017] (2) The catalyst precursor A obtained in step (1) is impregnated with an impregnation solution containing a Group VIII metal salt and an organic additive, and then dried and calcined to obtain a catalyst precursor B.

[0018] (3) The catalyst precursor B of step (2) is mixed with a molecular sieve precursor and subjected to hydrothermal treatment, followed by drying and calcining to obtain the silicon capture catalyst.

[0019] Furthermore, the sulfide powder of the VIB group metal in step (1) is molybdenum sulfide and / or tungsten sulfide.

[0020] Furthermore, the peptizing agent and extrusion aid in step (1) are well known to those skilled in the art. As a more specific embodiment, the peptizing agent is selected from at least one of nitric acid, phosphoric acid or acetic acid, and the extrusion aid is selected from at least one of starch and polyethylene glycol.

[0021] Furthermore, the drying conditions of step (1) are: drying temperature of 90-200°C, and drying time of 3-6 hours; the roasting conditions are: in air or oxygen atmosphere, roasting temperature of 300-700°C, and roasting time of 3-6 hours.

[0022] Furthermore, the Group VIII metal salt in step (2) is a nitrate, acetate or sulfate of a Group VIII metal, and an equal volume impregnation method can be adopted, and the Group VIII metal is Ni and / or Co.

[0023] Furthermore, the organic auxiliary agent in step (2) is an alcohol or organic acid containing hydroxyl and / or carboxyl groups, wherein the number of carbon atoms is 3-10. Specifically, it is at least one selected from ethylene glycol, glycerol, butanediol, pentanediol, acetic acid, citric acid, malonic acid, succinic acid and glutaric acid.

[0024] Furthermore, the drying conditions of step (2) are: drying temperature of 90-200°C, and drying time of 3-6 hours; and the roasting conditions are: in air or oxygen atmosphere, roasting temperature of 200-400°C, and roasting time of 3-6 hours.

[0025] Furthermore, the molecular sieve precursor in step (3) is a gel formed by mixing a silicon source and / or an aluminum source, a precipitant, a template and water, and its preparation method is well known to those skilled in the art, and adopts a precipitation or sol-gel method. The silicon source is generally one or more of sodium silicate, tetraethyl orthosilicate, silica sol and chromatography silica gel; the aluminum source is generally one or more of sodium aluminate, aluminum hydroxide and pseudo-boehmite; the precipitant is selected from at least one of sodium hydroxide, ammonia water and potassium hydroxide; the template is selected from one or more of hexadecyltrimethylammonium bromide, ethylenediamine, n-butylamine, tetrapropylammonium bromide, ethanol, tetraethylammonium hydroxide, tetraethylammonium bromide, triethylamine, di-n-propylamine, diisopropylamine and methylcellulose.

[0026] Furthermore, the hydrothermal treatment conditions in step (3) are: temperature of 90-200° C., pressure of 0.1-2.0 MPa, pH of 7.5-9.0, and time of 5-48 hours.

[0027] Furthermore, the drying conditions in step (3) are: drying temperature of 20-90°C, drying time of 4-16 hours; and roasting conditions are: in air or oxygen atmosphere, roasting temperature of 300-500°C, roasting time of 2-6 hours.

[0028] The technical purpose of the third aspect of the present invention is to provide the application of the silicon capture catalyst, which is used in the hydrogenation process of various silicon-containing raw materials such as coking dry gas, coking naphtha, coking diesel, etc.

[0029] Compared with the prior art, the catalyst of the present invention has the following advantages:

[0030] (1) The catalyst of the present invention is added with a molecular sieve, and the molecular sieve is loaded on the outer surface of the catalyst instead of being kneaded with the carrier. On the one hand, it is beneficial to increase the contact surface between the molecular sieve and the active metal, and to load the molecular sieve onto the active site of the active metal, thereby increasing the probability of the molecular sieve contacting with the cyclosiloxane compound and improving the ability of the molecular sieve to provide H protons for ring-opening reaction. The intermediate after ring opening then undergoes a hydrogenation desiliconization reaction with the active metal to fix silicon to the silicon-capturing catalyst, thereby improving the silicon-capturing ability of the catalyst. On the other hand, the ability of the molecular sieve to provide H protons can be accurately controlled by controlling the type and content of the molecular sieve, thereby regulating its activity. Thirdly, the utilization rate of the molecular sieve is increased, thereby reducing the amount of the molecular sieve used and reducing the cost of the catalyst.

[0031] (2) In the preparation method of the present invention, low-cost molybdenum sulfide powder and alumina powder are extruded into strips, and the molybdenum sulfide is converted into molybdenum oxide after calcination. The released sulfur trioxide can reduce the interaction between molybdenum oxide and alumina, and at the same time, a large number of pores can be generated, thereby increasing the pore volume and specific surface area of ​​the carrier and improving the silicon capacity of the catalyst. Then, the catalyst is impregnated with a mixed solution of a Group VIII metal and an organic additive, which is beneficial to weakening the interaction between the carrier and the active metal and improving the dispersion of the metal, and is also beneficial to loading the carrier onto the surface of the Group VIB metal oxide, thereby improving the hydrogenation activity of the catalyst.

[0032] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0033] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0034] The composition of the catalyst provided by the present invention is characterized by combining inductively coupled plasma ICP and XPS energy spectrum. First, the total content of the VIB group metal and the total content of the VIII group metal in the catalyst are characterized by ICP, and then the content of metal elements of different valence states in the catalyst is quantitatively characterized by XPS energy spectrometer.

[0035] The present invention uses CO-FTIR (carbon monoxide in-situ infrared analysis) to analyze the content of Group VIII metal oxides on Group VIB metal oxide wafers. The measurement conditions of the CO-FTIR include: after the catalyst is ground, it is pressed into a Φ13mm self-supporting sheet and placed on the in-situ pool sample holder. 3.0% H2S is used for sulfurization treatment at 320°C for 3h, then the temperature is lowered to room temperature in an H2S atmosphere, and then vacuumed to 300°C for purification for 2h, and CO adsorption is performed under the condition of lowering the temperature with liquid nitrogen. A small amount of CO gas is introduced into the in-situ pool, and after adsorption equilibrium for 30 minutes, it is desorbed to 10 -4Pa. The infrared spectra before and after the adsorption of CO were collected, and the difference between the two spectra was the infrared spectrum result of the catalyst adsorbing CO. The experiment used Nicolet 6700 Fourier transform infrared spectrometer, with 32 scans and a resolution of 4 cm -1 , 4000~650cm -1 Measurement, detector is MCT / A.

[0036] Example 1

[0037] (1) Molybdenum sulfide is mixed evenly with aluminum oxide powder, nitric acid, starch and deionized water, wherein the mass ratio of molybdenum sulfide: aluminum oxide powder: nitric acid: starch: deionized water is 7:93:4:3:60, and then kneaded and extruded into strips, and then dried at 110°C for 3 hours and calcined at 550°C for 3 hours to obtain catalyst precursor A.

[0038] (2) Impregnating the nickel nitrate and glycerol solution into the catalyst precursor A prepared in step (1), and then drying at 110°C for 3 hours and calcining at 350°C for 3 hours to obtain catalyst precursor B.

[0039] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(ethylenediamine):n(H2O)=15:1:7:4:190, and stirred to form a uniform sol, i.e., a precursor of Y molecular sieve, and then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, pH=8.0 for 10 h; then filtered, washed three times with deionized water, dried at 120°C for 3 h, and calcined at 450°C for 3 h to obtain silicon capture catalyst C-1.

[0040] The weight percentages of the components in the silicon capture catalyst C-1 are: MoO3 is 6.3%, NiO is 4.1%, Y molecular sieve is 3.1%, and the rest is alumina carrier.

[0041] Example 2

[0042] (1) Molybdenum sulfide is mixed evenly with aluminum oxide powder, nitric acid, starch and deionized water, wherein the mass ratio of molybdenum sulfide: aluminum oxide powder: nitric acid: starch: deionized water is 9:91:4:3:60, and then kneaded and extruded into strips, and then dried at 110°C for 3 hours and calcined at 450°C for 3 hours to obtain catalyst precursor A.

[0043] (2) Impregnating nickel nitrate and ethylene glycol solution into the catalyst precursor A prepared in step (1), then drying at 110°C for 3 hours and calcining at 250°C for 3 hours to obtain catalyst precursor B.

[0044] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(n-butylamine):n(H2O)=18:1:6:6:200, and stirred to form a uniform sol, i.e., a precursor of the ZSM-5 molecular sieve, which is then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, and pH=8.0 for 10 h; then filtered, washed three times with deionized water, dried at 120°C for 3 h, and calcined at 550°C for 3 h to obtain a silicon capture catalyst C-2.

[0045] The weight percentages of the components in the silicon capture catalyst C-2 are: MoO3 is 8.1%, NiO is 4.6%, ZSM-5 molecular sieve is 4.8%, and the rest is alumina carrier.

[0046] Example 3

[0047] (1) Molybdenum sulfide is mixed evenly with aluminum oxide powder, nitric acid, starch and deionized water, wherein the mass ratio of molybdenum sulfide: aluminum oxide powder: nitric acid: starch: deionized water is 10:90:4:3:60, and then kneaded and extruded into strips, and then dried at 110°C for 3 hours and calcined at 450°C for 3 hours to obtain catalyst precursor A.

[0048] (2) Impregnating nickel nitrate and ethylene glycol solution into the catalyst precursor A prepared in step (1), and then drying at 110°C for 3 hours and calcining at 450°C for 3 hours to obtain catalyst precursor B.

[0049] (3) Sodium aluminate and sodium hydroxide were dissolved in deionized water, and then tetraethylammonium bromide was added. The mixture was stirred vigorously, and silica sol was slowly added dropwise. The mixture was aged for 3 h, wherein the molar ratio of each component was n(SiO2):n(Al2O3):n(Na2O):n(tetraethylammonium bromide):n(H2O)=24:1:6:5.5:280, to form a precursor of a β-type molecular sieve. The precursor was then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, and pH=8.0 for 10 h. The mixture was then filtered, washed three times with deionized water, dried at 120°C for 3 h, and calcined at 550°C for 3 h to obtain a silicon capture catalyst C-3.

[0050] The weight percentages of the components in the silicon capture catalyst C-3 are: MoO3 is 9.6%, NiO is 4.8%, β-type molecular sieve is 5.0%, and the rest is alumina carrier.

[0051] Example 4

[0052] (1) Molybdenum sulfide is mixed evenly with aluminum oxide powder, nitric acid, starch and deionized water, wherein the mass ratio of molybdenum sulfide: aluminum oxide powder: nitric acid: starch: deionized water is 4:96:4:3:60, and then kneaded and extruded into strips, and then dried at 150° C. for 3 hours and calcined at 500° C. for 3 hours to obtain catalyst precursor A.

[0053] (2) Impregnating the nickel nitrate and glycerol solution into the catalyst precursor A prepared in step (1), and then drying at 90°C for 3 hours and calcining at 250°C for 3 hours to obtain the catalyst precursor B.

[0054] (3) Hexadecyltrimethylammonium bromide and sodium hydroxide are mixed and then added to deionized water. After stirring, ethyl orthosilicate is added dropwise to the mixed solution. After stirring for 30 minutes, the molar ratio of each component is n(SiO2):n(Na2O):n(hexadecyltrimethylammonium bromide):n(H2O)=12:2:4:200 to form an MCM-41 molecular sieve precursor, which is then mixed with the catalyst precursor B prepared in step (2) and then hydrothermally treated at 150°C, 1.0 MPa, and pH=8.0 for 10 hours; then filtered, washed with deionized water three times, dried at 120°C for 3 hours, and calcined at 500°C for 3 hours to obtain a silicon capture catalyst C-4.

[0055] The weight percentages of the components in the silicon capture catalyst C-4 are: MoO3 is 3.7%, NiO is 2.1%, MCM-41 molecular sieve is 3.4%, and the rest is alumina carrier.

[0056] Example 5

[0057] (1) Molybdenum sulfide is mixed evenly with aluminum oxide powder, nitric acid, starch and deionized water, wherein the mass ratio of molybdenum sulfide: aluminum oxide powder: nitric acid: starch: deionized water is 8:92:4:3:60, and then kneaded and extruded into strips, and then dried at 120°C for 3 hours and calcined at 450°C for 3 hours to obtain catalyst precursor A.

[0058] (2) The cobalt nitrate and citric acid solution is impregnated into the catalyst precursor A prepared in step (1), and then dried at 80°C for 3 hours and calcined at 350°C for 3 hours to obtain the catalyst precursor B.

[0059] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(ethylenediamine):n(H2O)=15:1:7:4:190, and stirred to form a uniform sol, i.e., a precursor of Y molecular sieve, and then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, pH=8.0 for 10 h; then filtered, washed three times with deionized water, dried at 120°C for 3 h, and calcined at 550°C for 3 h to obtain silicon capture catalyst C-5.

[0060] The weight percentages of the components in the silicon capture catalyst C-5 are: MoO3 is 7.8%, CoO is 4.1%, Y-type molecular sieve is 4.8%, and the rest is alumina carrier.

[0061] Example 6

[0062] (1) Tungsten sulfide is mixed evenly with alumina powder, nitric acid, starch and deionized water, wherein the mass ratio of molybdenum sulfide: alumina powder: nitric acid: starch: deionized water is 9:91:4:3:60, and then kneaded and extruded into strips, and then dried at 110°C for 3 hours and calcined at 520°C for 3 hours to obtain catalyst precursor A.

[0063] (2) Impregnating nickel nitrate and ethylene glycol solution into the catalyst precursor A prepared in step (1), then drying at 90°C for 3 hours and calcining at 200°C for 3 hours to obtain catalyst precursor B.

[0064] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(n-butylamine):n(H2O)=18:1:6:6:200, and stirred to form a uniform sol, i.e., a precursor of the ZSM-5 molecular sieve, which is then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, and pH=8.0 for 10 h; then filtered, washed three times with deionized water, dried at 120°C for 3 h, and calcined at 550°C for 3 h to obtain a silicon capture catalyst C-6.

[0065] The weight percentages of the components in the silicon capture catalyst C-6 are: WO3 is 8.6%, NiO is 4.2%, ZSM-5 molecular sieve is 4.8%, and the rest is alumina carrier.

[0066] Example 7

[0067] (1) Tungsten sulfide is mixed evenly with alumina powder, nitric acid, starch and deionized water, wherein the mass ratio of molybdenum sulfide: alumina powder: nitric acid: starch: deionized water is 8.2:91.8:4:3:60, and then kneaded and extruded into strips, and then dried at 120°C for 3 hours and calcined at 450°C for 3 hours to obtain catalyst precursor A.

[0068] (2) Impregnating the cobalt nitrate and glycerol solution into the catalyst precursor A prepared in step (1), and then drying at 100°C for 3 hours and calcining at 350°C for 3 hours to obtain the catalyst precursor B.

[0069] (3) Sodium hydroxide, silica sol, sodium aluminate and ethylenediamine are added to deionized water, wherein the molar ratio of each component is n(SiO2):n(Al2O3):n(Na2O):n(ethylenediamine):n(H2O)=15:1:7:4:190, and stirred to form a uniform sol, i.e., a precursor of Y molecular sieve, and then mixed with the catalyst precursor B prepared in step (2), and then hydrothermally treated at 150°C, 1.0 MPa, pH=8.0 for 10 h; then filtered, washed three times with deionized water, dried at 120°C for 3 h, and calcined at 520°C for 3 h to obtain silicon capture catalyst C-7.

[0070] The weight percentages of the components in the silicon capture catalyst C-7 are: WO3 is 7.9%, CoO is 4.2%, Y-type molecular sieve is 4.8%, and the rest is alumina carrier.

[0071] Comparative Example 1

[0072] (1) Mix Y-type molecular sieve with alumina powder, nitric acid, starch and deionized water, wherein the mass ratio of Y-type molecular sieve: alumina powder: nitric acid: starch: deionized water is 8:92:4:3:60, and then knead and extrude into strips, and then dry at 80°C for 10 hours and calcine at 650°C for 3 hours to obtain a modified alumina carrier.

[0073] (2) A mixed solution of phosphomolybdic acid and nickel nitrate was impregnated into the modified alumina carrier prepared in step (1), and then dried at 120°C for 3 hours and calcined at 450°C for 3 hours to obtain a silicon capture catalyst DC-1.

[0074] The weight percentages of the components in the catalyst DC-1 are: MoO3 is 8.1%, NiO is 4.8%, the Y molecular sieve content is 4.8%, and the rest is alumina.

[0075] Comparative Example 2

[0076] (1) Mixing Y-type molecular sieve with molybdenum oxide, aluminum oxide powder, nitric acid, starch and deionized water in a mass ratio of 4.8:8.1:87.1:4:3:60, kneading and extruding into strips, drying at 80°C for 10 hours, and calcining at 650°C for 3 hours to obtain a catalyst precursor.

[0077] (2) The nickel nitrate solution was impregnated into the catalyst precursor prepared in step (1), and then dried at 90° C. for 3 hours and calcined at 250° C. for 3 hours to obtain the silicon capture catalyst DC-2.

[0078] The weight percentages of the components in the catalyst DC-2 are: MoO3 is 7.7%, NiO is 4.2%, Y molecular sieve is 4.6%, and the rest is alumina.

[0079] The content of Group VIII metal oxide on the Group VIB metal oxide wafers and the physicochemical properties of the catalysts C-1 to C-7 prepared in the above examples and the catalysts DC-1 to DC-2 prepared in the comparative examples were analyzed. The analysis results are shown in Table 1.

[0080] Table 1.

[0081]

[0082] Example 8

[0083] This example illustrates the silicon-capturing activity of the catalyst provided by the present invention on coker naphtha.

[0084] The evaluation raw oil used is coking naphtha raw material provided by a refinery of Sinopec, and its main properties are as follows: sulfur content is 5460μg / g, nitrogen content is 246μg / g, and silicon content is 38μg / g. A 200mL fixed bed hydrogenation device was used to evaluate the silicon capture capacity of catalysts C-1 to C-7 and comparative examples DC-1 to DC-2. Catalysts C-1 to C-7 and comparative examples DC-1 and DC-2 were pre-sulfurized. The pre-sulfurization conditions are: using aviation kerosene containing 3wt% CS2 at an air velocity of 1.5h -1 , hydrogen / oil volume ratio 500:1, presulfurization was carried out at an operating pressure of 4.0MPa. The evaluation reaction conditions were: operating pressure 3.0MPa, reaction temperature 260℃, hydrogen / oil volume ratio 200:1, volume space velocity 6.0h -1 The evaluation results are shown in Table 2.

[0085] Table 2.

[0086]

[0087] It can be seen from Table 2 that the silicon-capturing catalyst of the present invention not only has a high silicon-capturing capacity, but also has a high hydrogenation activity.

Claims

1. A silicon capture catalyst, characterized in that: The catalyst uses alumina as a carrier, on which molecular sieves and active components are loaded. The active components are oxides of metals of Group VIB and oxides of metals of Group VIII. Based on the total weight of the catalyst, the molecular sieve accounts for 1-12wt%, the metals of Group VIB account for 2-15% in terms of oxide, and the metals of Group VIII account for 2-10% in terms of oxide. The content of the metal oxides of Group VIII on the metal oxide wafers of Group VIB accounts for 60-100% of the content of the metal oxides of Group VIII. The molecular sieve is loaded on the outer surface of the catalyst; The silicon capture catalyst is prepared by the following method: (1) Alumina powder, sulfide powder of Group VIB metal, peptizing agent and extrusion aid are mixed, extruded into strips, and dried and calcined to obtain catalyst precursor A; (2) impregnating the catalyst precursor A of step (1) with an impregnation solution containing a Group VIII metal salt and an organic additive, and obtaining a catalyst precursor B through drying and calcination; (3) The catalyst precursor B of step (2) is mixed with a molecular sieve precursor and subjected to hydrothermal treatment, followed by drying and calcining to obtain the silicon capture catalyst.

2. The silicon-trapping catalyst according to claim 1, characterized in that: Based on the total weight of the catalyst, the molecular sieve accounts for 1.5-8wt%, the Group VIB metal accounts for 5-10% in terms of oxide, and the Group VIII metal accounts for 2-10% in terms of oxide.

3. The silicon-trapping catalyst according to claim 2, characterized in that: Based on the total weight of the catalyst, the molecular sieve accounts for 2-6 wt%.

4. The silicon-trapping catalyst according to claim 1, characterized in that: The pore volume of the silicon capture catalyst is 0.5-1.0 mL / g, and the specific surface area is 250-500 m 2 / g, the acid content of B is 0.05-0.3mmol / g.

5. The silicon-trapping catalyst according to claim 1, characterized in that: When the silicon-trapping catalyst is analyzed by CO-FTIR, the molar ratio of the Group VIB metal-Group VIII metal-S phase to the Group VIII metal is 60-100%.

6. The silicon-trapping catalyst according to claim 5, characterized in that: When the silicon-capturing catalyst is analyzed by CO-FTIR, the molar ratio of the VIB group metal-VIII group metal-S phase to the VIII group metal is 65%-90%.

7. The silicon-trapping catalyst according to claim 1, characterized in that: The molecular sieve is at least one selected from Y-type molecular sieve, ZSM-5 molecular sieve, β-type molecular sieve and MCM-41 molecular sieve.

8. The silicon-trapping catalyst according to claim 1, characterized in that: The VIB group metal oxide is molybdenum trioxide and / or tungsten trioxide, and the VIII group metal oxide is nickel oxide and / or cobalt oxide.

9. The method for preparing the silicon trapping catalyst according to claim 1, comprising the following steps: (1) Alumina powder, sulfide powder of Group VIB metal, peptizing agent and extrusion aid are mixed, extruded into strips, and dried and calcined to obtain catalyst precursor A; (2) impregnating the catalyst precursor A of step (1) with an impregnation solution containing a Group VIII metal salt and an organic additive, and obtaining a catalyst precursor B through drying and calcination; (3) The catalyst precursor B of step (2) is mixed with a molecular sieve precursor and subjected to hydrothermal treatment, followed by drying and calcining to obtain the silicon capture catalyst.

10. The preparation method according to claim 9, characterized in that: The sulfide powder of the VIB group metal in step (1) is molybdenum sulfide and / or tungsten sulfide.

11. The preparation method according to claim 9, characterized in that: The peptizing agent is selected from at least one of nitric acid, phosphoric acid or acetic acid, and the extrusion aid is selected from at least one of starch and polyethylene glycol.

12. The preparation method according to claim 9, characterized in that: The drying conditions of step (1) are: drying temperature of 90-200°C, and drying time of 3-6 hours; the roasting conditions are: in air or oxygen atmosphere, roasting temperature of 300-700°C, and roasting time of 3-6 hours.

13. The preparation method according to claim 9, characterized in that: The Group VIII metal salt in step (2) is a nitrate, acetate or sulfate of a Group VIII metal.

14. The preparation method according to claim 9, characterized in that: The organic auxiliary agent in step (2) is at least one selected from ethylene glycol, propylene glycol, butylene glycol, pentanediol, acetic acid, citric acid, malonic acid, succinic acid and glutaric acid.

15. The preparation method according to claim 9, characterized in that: The drying conditions of step (2) are: drying temperature of 90-200°C, and drying time of 3-6 hours; the roasting conditions are: roasting temperature of 200-400°C, and roasting time of 3-6 hours in air or oxygen atmosphere.

16. The preparation method according to claim 9, characterized in that: The molecular sieve precursor described in step (3) is a gel formed by mixing a silicon source and / or an aluminum source, a precipitant, a template and water, and the molecular sieve is obtained by precipitation or sol-gel method.

17. The preparation method according to claim 9, characterized in that: The hydrothermal treatment conditions in step (3) are: temperature of 90-200° C., pressure of 0.1-2.0 MPa, pH of 7.5-9.0, and time of 5-48 hours.

18. The preparation method according to claim 9, characterized in that: The drying conditions in step (3) are: drying temperature of 20-90°C, and drying time of 4-16 hours; the roasting conditions are: in air or oxygen atmosphere, roasting temperature of 300-500°C, and roasting time of 2-6 hours.

19. Use of the silicon-capturing catalyst according to claim 1, which is used in the hydrogenation process of various silicon-containing raw materials such as coking dry gas, coking naphtha, and coking diesel.