A catalyst for amination reaction and its preparation method and application

The alumina structure is converted by high-temperature pre-baking and combined with Hβ molecular sieve and metal loading to adjust the acid amount of the catalyst, solving the problems of carbon deposition and poor stability of the ammonia catalyst due to its high acidity, and achieving the stability and operation cycle of the catalyst. improvement.

CN116060100BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111278629.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-31
Publication Date
2024-10-01
Estimated Expiration
2041-10-31

AI Technical Summary

Technical Problem

The existing ammonia catalyst has problems such as carbon deposition and blockage in the ammonia reaction due to its high acidity, decreased reaction activity, poor stability, and short single-pass operation cycle.

Method used

By converting pseudo-boehmite into delta, theta or alpha alumina by pre-baking at high temperature, and combining it with Hβ molecular sieve and metal loading, the acid amount and acid distribution of the catalyst can be adjusted, the acid density can be reduced, and a suitable acid can be formed. Strength and acidity.

Benefits of technology

Significantly improves the stability and single-pass operation cycle of the catalyst, and extends the service life of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116060100B_ABST
    Figure CN116060100B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method for an amination reaction catalyst. The method comprises: (1) pre-baking pseudo-boehmite at a temperature of 800°C to 1200°C to obtain a single crystal or composite crystal aluminum oxide; (2) metal-modifying the Hβ molecular sieve by an impregnation method, followed by filtering, drying and calcining; (3) fully kneading the modified Hβ molecular sieve obtained in step (2), the aluminum oxide obtained in step (1), an extrusion aid and a peptizing agent solution in a certain proportion, forming, and then drying and calcining to obtain an Hβ molecular sieve catalyst. The catalyst prepared by the method has a suitable acid strength and acid amount, and the catalyst stability is significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an amination reaction catalyst, a preparation method and application thereof, in particular to a molecular sieve catalyst, a preparation method and application thereof. Background Art

[0002] Amination reaction is an important chemical reaction in the chemical industry, such as the preparation of tert-butylamine by amination of isobutylene, the synthesis of diphenylamine by aniline, the preparation of hexamethylenediamine by amination of hexamethylenediol, etc. At present, the amination catalysts introduced in domestic and foreign patent technologies are mostly solid acid catalysts, such as US3118944, US4454348, US3944613, CN94107296.7 and other patents disclose the technology of using activated alumina, amorphous silicon aluminum, and molecular sieves to prepare catalysts. In the mid-1990s, my country successfully developed a new process for the continuous synthesis of diphenylamine from aniline and a matching special molecular sieve catalyst.

[0003] Amination is an acid-catalyzed reaction. The acid properties of the catalyst directly affect the reaction activity, selectivity and stability. One of the main causes of catalyst deactivation is carbon deposition. The complex reactants, products and by-products undergo a graphitization reaction with an increase in carbon number on the acid center. The catalyst blocks the pores due to carbon deposition, and the reactants cannot diffuse into the pores to contact the acid center, resulting in a decrease in catalyst activity. The products cannot diffuse out of the pores, which intensifies the graphitization reaction process.

[0004] To solve this problem, methods of adjusting the acid properties and pore structure of molecular sieves are often used. For example, CN1289642A and CN1951564A describe that in the process of continuous preparation of diphenylamine from aniline in liquid phase, the catalyst composed of Hβ molecular sieve and alumina used has been improved. Alkaline earth metals and alkali metals are added to the catalyst respectively to adjust the acid center of the catalyst, reduce the strong acid center on the catalyst that is prone to polymerization reaction, and improve the aniline conversion rate and diphenylamine selectivity. CN105618106B uses multi-level pore Beta molecular sieve as a catalyst. The increase in pore volume and pore size changes the diffusion behavior of reactants and products, increases the carbon capacity of the catalyst, and improves the catalyst single-pass operation cycle.

[0005] The existing industrially applied amination catalyst is made by mixing and kneading molecular sieve and pseudo-boehmite into strips and then calcining them. The molecular sieve provides most of the active centers, and alumina is used as a binder. After calcination, it is generally γ-type. Alumina is also a solid acid with a large number of acid centers. The amination reaction can also occur on alumina used as a binder. For example, patents US3118944 and US4454348 use pure alumina as a catalyst to synthesize diphenylamine from aniline. Alumina has a high acid content and a high acid density. The reactants are very likely to undergo graphitization reactions such as cyclization and polymerization on such a high-density acid center, resulting in an increase in the amount of carbon deposits on the catalyst, blocking the catalyst pores and causing the catalyst to deactivate, resulting in poor catalyst stability and a short single-pass operation cycle. Summary of the invention

[0006] In view of the shortcomings of the prior art, the first aspect of the present invention provides a method for preparing an amination reaction catalyst. The amination catalyst prepared by the method has suitable acid strength and acid amount, and the catalyst stability is significantly improved.

[0007] A method for preparing an amination reaction catalyst comprises the following steps:

[0008] (1) Pre-calcining pseudo-boehmite at a temperature of 800°C to 1200°C to obtain single crystal or composite crystal alumina;

[0009] (2) The Hβ molecular sieve is metal-modified by an impregnation method, followed by filtration, drying and calcination;

[0010] (3) The modified Hβ molecular sieve obtained in step (2), the alumina obtained in step (1), the extrusion aid and the peptizing agent solution are fully kneaded in a certain proportion, molded, and then dried and calcined to obtain an Hβ molecular sieve catalyst.

[0011] Furthermore, the temperature of the pseudo-boehmite pre-baking in step (1) is preferably 850°C to 1150°C; the baking time is generally 1h to 10h, preferably 2h to 6h. The alumina obtained after pre-baking has a single crystal structure of δ-type, θ-type or α-type, or a composite structure of the above two crystal types.

[0012] Furthermore, the silicon-aluminum (SiO2 / Al2O3) molar ratio of the Hβ molecular sieve in step (2) is 20-300, preferably 30-200. The metal is selected from at least one of Li, Na, K, Mg, Ca, Sr, La, Ce, Pr, Zr, and Cu, preferably Na or Mg. The metal precursor used is a nitrate or chloride of the metal. Step (2) needs to be filtered, dried, and calcined after impregnation. The impregnation, filtration, drying, and calcination processes are well known to those skilled in the art. The amount of metal added in terms of oxide is 0.1% to 5.0% by weight of the finished catalyst, preferably 0.3% to 4.6%.

[0013] Furthermore, the operation of step (3) is well known to those skilled in the art. For example, the weight ratio of the Hβ molecular sieve (on a dry basis), alumina, extrusion aid and peptizing agent is 100: (15-50): (3-20): (5-80), preferably 100: (20-35): (10-15): (20-50). In the amount of materials used, the amount of Hβ molecular sieve is the weight on a dry basis.

[0014] Furthermore, the extrusion aid may be selected from sesbania powder. The peptizing agent may be selected from dilute nitric acid solution or citric acid. The mass concentration of the dilute nitric acid solution is generally 3% to 15%.

[0015] Furthermore, the drying conditions of step (3) are as follows: the drying temperature is 60°C to 150°C, preferably 80°C to 120°C, and the drying time is 8h to 24h, preferably 10h to 20h. Step (3) is preferably dried in the shade for 10h to 48h before drying. The roasting conditions are as follows: the roasting temperature is 300°C to 800°C, preferably 400°C to 700°C, and the roasting time is 2h to 24h, preferably 4h to 8h.

[0016] Furthermore, in step (3), precursors such as Si, P, B, and C can be selectively added. The amount of catalyst acid and acid distribution can be adjusted to improve the size of catalyst pores and pores. Furthermore, the Hβ molecular sieve catalyst obtained by the method of the present invention includes, based on the weight of the catalyst:

[0017] Hβ molecular sieve 50%~85%, preferably 65%~80%;

[0018] The metal is 0.1% to 5% in terms of oxide, preferably 0.3% to 4.6%;

[0019] Alumina 10%~45%, preferably 15%~34.5%;

[0020] The silicon-aluminum molar ratio of the Hβ molecular sieve is 20-300, preferably 30-200.

[0021] Further, the acid amount distribution of the obtained Hβ molecular sieve catalyst is: the weak acid amount is 0.45~0.65mmol / g, the medium strong acid amount is 0.25~0.4mmol / g, and the strong acid amount is 0.05~0.2mmol / g. Preferably, the weak acid amount is 0.48~0.60mmol / g, the medium strong acid amount is 0.28~0.38mmol / g, and the strong acid amount is 0.08~0.15mmol / g. In the present invention, weak acid refers to an acid center with an NH3 desorption temperature of 150℃~250℃ when using NH3-TPD to characterize the acid distribution of the catalyst, medium strong acid refers to an acid center with an NH3 desorption temperature of 250℃~400℃, and strong acid refers to an acid center with an NH3 desorption temperature of 400℃~500℃. Further, the Hβ molecular sieve catalyst is a strip or spherical particle. The cross section of the strip particles can be cylindrical, clover or four-leaf grass, with a diameter of 0.5~3.0mm, preferably 1.0~2.0mm; the diameter of the spherical particles is 0.5~5.0mm, preferably 1.0~3.0mm. The specific surface area of ​​the catalyst is generally 300~600m 2 / g, preferably 400~550m 2 / g; the specific pore volume is generally 0.25~0.50mL / g, preferably 0.30~0.45mL / g; the average pore diameter is generally 1.5~5nm, preferably 2.0~4.0nm.

[0022] Furthermore, the metal is selected from at least one of Li, Na, K, Mg, Ca, Sr, La, Ce, Pr, Zr, and Cu, preferably Na or Mg.

[0023] Furthermore, the aluminum oxide is a δ-type, θ-type or α-type single crystal structure, or a composite structure of the above two crystal types.

[0024] The present invention also provides an amination reaction, in which the Hβ molecular sieve catalyst prepared above is used.

[0025] Furthermore, the amination reaction includes amination reactions of other olefins and alcohols such as amination of isobutylene to produce tert-butylamine, amination of aniline to synthesize diphenylamine, amination of 1,3-propylene glycol to produce 1,3-propylenediamine, etc.

[0026] Furthermore, the amination reaction comprises the following contents: the reaction raw materials containing amines or liquid ammonia are passed through a fixed bed reactor containing an Hβ molecular sieve catalyst, and the amination reaction is carried out under reaction conditions.

[0027] Furthermore, the reaction feeding method can be top feeding or bottom feeding. The reaction conditions are: reaction temperature is 100~500℃, reaction pressure (gauge pressure) is 1~6 MPa, raw material (in terms of amines or liquid ammonia) volume space velocity is 0.1~5 h -1During the reaction, hydrogen or nitrogen can be introduced as a carrier gas, or the reaction can be carried out without a carrier gas.

[0028] When the applicant studied the amination reaction and its catalyst, he came to the following conclusion: the amination reaction is an acid-catalyzed reaction. The existing industrially applied amination catalyst is made by mixing and kneading molecular sieves and pseudo-boehmite into strips and then calcining them. The molecular sieve provides most of the active centers. Alumina is used as a binder. After calcination, it is generally γ-type and has a large number of acid centers. The amination reaction can also occur on the alumina used as a binder. The acid content of γ-type alumina is relatively high, which further increases the acid density. The reactants are very likely to undergo graphitization reactions such as cyclization and polymerization on such a high-density acid center, resulting in an increase in the amount of carbon deposits on the catalyst, blocking the catalyst pores and causing the catalyst to deactivate. However, the simple method of loading metals to adjust the acidity has limited effect. Therefore, the inventor of the present application was inspired by this: in the amination catalyst composed of molecular sieves and alumina, in addition to the existing acidity (acidity) adjustment means, the acid properties of alumina can also be effectively adjusted to obtain better catalytic performance. However, there are few such reports in the existing technology center.

[0029] In the method of the present invention, the precursor of the binder aluminum oxide, pseudo-boehmite, is pre-calcined at a temperature far higher than the normal conditions, so that it is pre-crystallized into a single crystal structure of δ type, θ type or α type or a composite structure of the two crystal types, which can greatly reduce the total acid content of the aluminum oxide, especially the acid density. The aluminum oxide after crystallization is then kneaded with molecular sieves and loaded with metals to obtain a finished catalyst, which has a low total acid content, good stability and a long single-pass operation cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the XRD spectrum of alumina after pre-calcination in Example 1. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is described in detail below in conjunction with embodiments, but the present invention is not limited to the following embodiments.

[0032] Example 1

[0033] Pseudo-boehmite was calcined at 950°C for 5 hours to transform into θ+δ type alumina. Hβ molecular sieve with a silicon-aluminum ratio of 50 was loaded with Na by impregnation, and then filtered, dried and calcined.

[0034] The pretreated Hβ molecular sieve (dry basis), alumina, sesbania powder and dilute nitric acid solution (10wt%) were mixed evenly in a mass ratio of 75:25:3:55 and extruded into strips, then dried in the shade for 24 hours, dried in an oven at 110°C for 24 hours, and calcined at 550°C for 4 hours to obtain a finished catalyst, recorded as A. The catalyst composition is: Hβ molecular sieve content 72.9%, sodium oxide content 2.8%, and alumina 24.3%.

[0035] Comparative Example 1

[0036] The catalyst preparation scheme is similar to that of Example 1, except that the catalyst is formed by mixing and kneading unprecalcined pseudo-boehmite with Hβ molecular sieve with a Na-loaded silicon-aluminum ratio of 50, sesbania powder, etc. The obtained catalyst is recorded as B1, and the catalyst composition is: Hβ molecular sieve content 72.9%, sodium oxide content 2.8%, aluminum oxide 24.3%.

[0037] Comparative Example 2

[0038] Referring to Chinese patent CN1951564A, Hβ molecular sieve catalyst was prepared, and the catalyst was recorded as B2.

[0039] Example 2

[0040] Pseudo-boehmite was calcined at 1050°C for 6 hours to transform into θ-type alumina. Hβ molecular sieve with a silicon-aluminum ratio of 75 was loaded with Na and La by impregnation, and then filtered, dried and calcined.

[0041] The pretreated Hβ molecular sieve, alumina, sesbania powder and dilute nitric acid solution (10wt%) were mixed uniformly in a mass ratio of 80:20:4:55 and then extruded into strips, then dried in the shade for 24 hours, dried in an oven at 110°C for 16 hours, and calcined at 540°C for 4 hours to obtain a finished catalyst, recorded as C. The catalyst composition is: Hβ molecular sieve content 78.1%, sodium oxide content 1.9%, lanthanum oxide content 0.5%, and alumina 19.5%.

[0042] Example 3

[0043] Pseudo-boehmite was calcined at 1000°C for 4 hours to transform into θ+δ type alumina. Hβ molecular sieve with a silicon-aluminum ratio of 85 was loaded with Mg and Ce by impregnation, and then filtered, dried and calcined.

[0044] The pretreated Hβ molecular sieve, alumina, sesbania powder and dilute nitric acid solution (10wt%) were mixed uniformly in a mass ratio of 70:30:5:60 and then extruded into strips, then dried in the shade for 24 hours, dried in an oven at 120°C for 24 hours, and calcined at 560°C for 4 hours to obtain a finished catalyst, denoted as D. The catalyst composition is: Hβ molecular sieve content 68.0%, magnesium oxide content 2.0%, cerium oxide content 0.8%, and aluminum oxide 29.2%.

[0045] Example 4

[0046] The catalysts prepared in the above embodiments and comparative examples were used to conduct an evaluation experiment of aniline to diphenylamine in a micro-evaluation device. Aniline was used as the raw material, the initial reaction temperature was 300°C, and when the aniline conversion rate dropped below 20%, the reaction temperature was increased, the pressure was 3.0 MPa, and the volumetric space velocity of aniline was 0.25 h -1 The data after 2 hours and 1700 hours of operation are listed in Table 1, and the acid distribution of the catalysts of various examples and comparative examples is listed in Table 2.

[0047] Table 1

[0048]

[0049] Table 2 (Unit: mmol / g)

[0050]

Claims

1. A method for preparing an amination reaction catalyst, comprising the following steps: (1) Pre-calcining pseudo-boehmite at a temperature of 800°C to 1200°C to obtain single crystal or composite crystal alumina; (2) The Hβ molecular sieve is metal-modified by an impregnation method, followed by filtration, drying and calcination; (3) The modified Hβ molecular sieve obtained in step (2), the alumina obtained in step (1), the extrusion aid and the peptizing agent solution are fully kneaded in a certain proportion, molded, and then dried and calcined to obtain an Hβ molecular sieve catalyst.

2. The preparation method according to claim 1, characterized in that: In step (1), the temperature of pre-baking the pseudo-boehmite is 850° C. to 1150° C., and the baking time is 1 h to 10 h.

3. The preparation method according to claim 1, characterized in that: The crystal form of the aluminum oxide obtained in step (1) is a single crystal structure of δ-type, θ-type or α-type, or a composite structure of the above two crystal forms.

4. The preparation method according to claim 1, characterized in that: The silicon-aluminum molar ratio of the Hβ molecular sieve in step (2) is 20-300.

5. The preparation method according to claim 1, characterized in that: The metal described in step (2) is selected from at least one of Li, Na, K, Mg, Ca, Sr, La, Ce, Pr, Zr and Cu; the amount of the metal added in terms of oxide is 0.1% to 5.0% of the weight of the catalyst.

6. The preparation method according to claim 5, characterized in that: The metal in step (2) is selected from Na or Mg.

7. The preparation method according to claim 1, characterized in that The weight ratio of the Hβ molecular sieve obtained in step (2), the alumina obtained in step (1), the extrusion aid and the peptizing agent is 100: (15-50): (3-20): (5-80).

8. The preparation method according to claim 1, characterized in that: The drying conditions in steps (2) and (3) are: drying temperature of 60°C to 150°C, and drying time of 8h to 24h; the roasting conditions are: roasting temperature of 300°C to 800°C, and roasting time of 2h to 24h.

9. The preparation method according to claim 1, characterized in that: In step (3), the precursors of Si, P, B and C are selectively added.

10. The Hβ molecular sieve catalyst obtained by the preparation method according to any one of claims 1 to 8, comprising, based on the weight of the catalyst: Hβ molecular sieve 50%~85%; Metals are 0.1% to 5% in terms of oxides; Alumina 10%~45%; Wherein, the silicon-aluminum molar ratio of the Hβ molecular sieve is 20-300.

11. The Hβ molecular sieve catalyst obtained by the preparation method according to claim 10, comprising, based on the weight of the catalyst: Hβ molecular sieve 65%~80%; Metals as oxides 0.3%~4.6%; Alumina 15%~34.5%; Wherein, the silicon-aluminum molar ratio of the Hβ molecular sieve is 30-200.

12. The Hβ molecular sieve catalyst according to claim 10, characterized in that The specific surface area of ​​the catalyst is 300~600m 2 / g, the specific pore volume is 0.25~0.50mL / g, and the average pore diameter is 1.5~5nm.

13. The Hβ molecular sieve catalyst according to claim 10 or 11, characterized in that: The metal is selected from at least one of Li, Na, K, Mg, Ca, Sr, La, Ce, Pr, Zr and Cu.

14. An amination reaction, characterized in that: The Hβ molecular sieve catalyst described in any one of claims 10 to 13 is used.

15. The amination reaction according to claim 14, characterized in that: The amination reaction includes the amination of isobutylene to produce tert-butylamine, the synthesis of diphenylamine from aniline, and the amination of 1,3-propylene glycol to produce 1,3-propylenediamine.

16. The amination reaction according to claim 14, characterized in that: The amination reaction comprises the following contents: reaction raw materials containing amines or liquid ammonia are passed through a fixed bed reactor containing an Hβ molecular sieve catalyst to carry out an amination reaction under reaction conditions.