A titanium alloy electrode integral forming density detection and control system and method
By detecting the density of titanium alloy electrodes online and dynamically adjusting the pressing parameters, the problem of uneven density of titanium alloy electrodes is solved and product quality is improved.
Patent Information
- Application Number
- CN202211731224.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-30
AI Technical Summary
During the hydraulic press pressing process of titanium alloy electrodes, due to human factors or changes in raw materials, the density of the overall titanium alloy electrodes is uneven, affecting the quality of the product.
An online detection and control system for the overall forming density of titanium alloy electrodes is designed. It uses a material barrel, a feeding device, a pressing rod, a weighing sensor, a displacement sensor and a PLC controller to adjust the holding pressure by measuring and calculating the electrode density in real time. Time, pressing rod speed and pressing stop position realize dynamic control of density.
It effectively ensures the uniformity of density of titanium alloy integrally formed electrodes, improves product quality, and ensures that the density is within the range of process requirements.
Smart Images

Figure CN116067830B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of titanium alloy material processing, and in particular relates to a titanium alloy electrode integral forming density detection and control system and method, which are applied to the preparation of titanium alloy vacuum consumable integral electrodes. Background Art
[0002] Titanium alloy refers to a variety of alloy metals made of titanium and other metals. It has the advantages of low density, high specific strength, high temperature resistance, low temperature resistance, corrosion resistance, weldability, non-magnetic, good biocompatibility, etc. It is the material with the highest strength, best heat resistance and best corrosion resistance among the three major light metals (Al, Mg, Ti). It is widely used in aviation, aerospace, ships, weapons, chemical industry and other fields. The market demand for integral forming of titanium alloy electrodes is becoming more and more extensive.
[0003] At present, in the process of hydraulic press pressing titanium alloy integral electrodes, the operator mainly inputs the pressing speed and other process parameters in the HMI human-machine interface to indirectly control the density of the pressed electrode. In actual production, the density of the pressed integral titanium alloy electrode may be uneven or out of tolerance due to human factors or changes in titanium alloy raw materials, resulting in unqualified product quality. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide a titanium alloy electrode integral forming density detection and control system and method.
[0005] To achieve the above objectives, the present invention provides a titanium alloy electrode integral forming density detection and control system, which adopts the following technical solutions:
[0006] A titanium alloy electrode integral forming density online detection and control system comprises a barrel, a feeding device, a press rod, a receiving device, a weighing sensor, a press rod displacement sensor and a receiving device displacement sensor, wherein the barrel is used to load titanium alloy raw materials; the feeding device is located outside the barrel and can enter above the barrel and add titanium alloy raw materials into the barrel; the weighing sensor is arranged on the feeding device and is used to measure the weight of the added titanium alloy raw materials; the press rod is located directly above the barrel and can extend into the barrel to press the titanium alloy raw materials in the barrel into titanium alloy integral electrodes, the press rod displacement sensor is arranged on the press rod, and the position of the lower surface of the pressed electrode is obtained by detecting the position of the press rod; a forming die is arranged directly below the barrel, the receiving device is located directly below the forming die, the receiving device displacement sensor is arranged on the receiving device, and the length of the pressed electrode is obtained by detecting the position of the receiving device, and the weighing sensor, the press rod displacement sensor and the receiving device displacement sensor are all connected to a PLC controller with electrical signals.
[0007] Furthermore, the diameter of the forming die opening is smaller than the diameter of the barrel.
[0008] Furthermore, the titanium alloy electrode overall forming density online detection and control system also includes an HMI human-machine interface, and the HMI human-machine interface is connected to the PLC controller via electrical signals.
[0009] Preferably, the press rod is connected to a PLC controller via an electrical signal, and the press rod can be adjusted via the PLC controller.
[0010] Furthermore, PCL calculates the density of the pressed titanium alloy electrode in real time by collecting data and integrating the barrel cross-sectional area and the forming die cross-sectional area input by the HMI human-machine interface, and adjusts the holding time, pressing rod pressing speed and pressing end position according to the density change.
[0011] Another aspect of the present invention is to provide a method for detecting and controlling the overall forming density of a titanium alloy electrode, which adopts the following technical solution:
[0012] A method for detecting and regulating the overall forming density of a titanium alloy electrode, using the online detection and regulation system for the overall forming density of a titanium alloy electrode, comprises the following steps:
[0013] Step 1: Input the barrel cross-sectional area S0 and the reference density ρ of the pressed whole electrode into the PLC controller. 基准 ;
[0014] Step 2: At the end of the previous cycle, before the press rod rises and returns, the PLC controller detects the position of the press rod through the press rod displacement sensor to obtain the overall electrode upper surface position L of the previous cycle. 10 ;
[0015] Step 3: The pressing rod rises and returns, and the feeding device is loaded. The PLC controller collects the weight m of the titanium alloy raw material in the feeding device through the weighing sensor. The feeding device enters the top of the barrel, pours all the titanium alloy raw materials into the barrel, and then returns to the outside of the barrel;
[0016] Step 4: The press rod descends and presses the whole electrode until the electrode is squeezed out from the outlet of the forming die, pushing the receiving device to move. When the displacement sensor of the receiving device detects that the position of the whole electrode changes, the PLC controller obtains the position L of the upper surface of the electrode at this time through the press rod displacement sensor. 11 ;
[0017] Step 5: The PLC controller calculates the data obtained in the above steps to obtain the density ρ1 of the pressed titanium alloy electrode and compares it with the reference density ρ 基准 For comparison:
[0018] If ρ1<ρ 基准, then, increase the holding time t of this pressing, increase the downward speed ν of the pressing rod, and increase the stopping position L of this cycle pressing 10 ;
[0019] If ρ1>ρ 基准 , then reduce the holding time t of this pressing, reduce the downward speed ν of the pressing rod, and reduce the stopping position L of this cycle pressing 10 ;
[0020] Step 6: The pressure rod maintains the pressure for the time t, speed ν and stop position L as described in step 5. 10 After the pressure is maintained, the whole electrode is pressed downwards, and the electrode is extruded from the outlet of the forming die, pushing the receiving device to continue to move downwards;
[0021] Step 7: Repeat the above cycle until the overall electrode of the required length is obtained.
[0022] Preferably, the barrel cross-sectional area S0 and the reference density ρ of the pressed whole electrode are input to the PLC controller through the HMI human-machine interface. 基准 .
[0023] Preferably, in step 1, the reference density ρ 基准 3.1~3.6g / cm 3 between.
[0024] Preferably, in step 5, the downward movement speed v of the pressing rod is between 1 and 10 mm / s. The reference density of the present invention is the electrode density required for pressing the electrode*the square of the mold diameter / the square of the barrel diameter;
[0025] Electrode density = titanium alloy raw material weight / barrel cross-sectional area * length of the electrode pressed in this cycle
[0026] Compared with the prior art, the present invention has the following beneficial effects: the present invention detects the density of the electrode being pressed online, and adjusts the holding time, pressing speed, and pressing stop position according to the measured electrode density, thereby adjusting the density of the pressed electrode, thereby ensuring that the density of the titanium alloy integrally formed electrode is within the range of process requirements, improving the density uniformity, and improving the product quality of the titanium alloy integrally formed electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0028] Figure 1 It is a schematic diagram of the titanium alloy electrode integral forming density detection and control system of the present invention;
[0029] Figure 2It is a schematic diagram of the method for detecting and controlling the overall forming density of the titanium alloy electrode of the present invention;
[0030] Markings in the figure: 1. Feeding device; 2. Weighing sensor; 3. Pressing rod; 4. Pressing rod displacement sensor; 5. Barrel; 6. Titanium alloy raw material; 7. Forming die; 8. Titanium alloy integral electrode; 9. Material receiving device; 10. Material receiving device displacement sensor; 11. PLC controller; 12. HMI human-machine interface. DETAILED DESCRIPTION
[0031] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0032] Example 1
[0033] like Figure 1 As shown, an online detection and control system for the overall forming density of a titanium alloy electrode comprises a feeding device 1, a pressing rod 3, a receiving device 9 and an HMI human-machine interface 12, wherein a weighing sensor 2 is arranged on the feeding device 1, and is used to measure the weight of the added titanium alloy raw material 6; a pressing rod displacement sensor 4 is arranged on the pressing rod 3, and the pressing rod displacement sensor 4 is used to obtain the position of the lower surface of the pressed electrode by detecting the position of the pressing rod 3 under a specific state; a receiving device displacement sensor 10 is arranged on the receiving device 9, and the length of the pressed electrode 8 is obtained by detecting the position of the receiving device 9. The weighing sensor 2, the pressing rod displacement sensor 4, the receiving device displacement sensor 10, and the HMI human-machine interface 12 are all electrically connected to the PLC controller 11; the barrel 5 is used to load the titanium alloy raw material 6; the feeding device 1 is located outside the barrel 5, and can enter the barrel 5 to add the titanium alloy raw material 6 into the barrel 5; the pressing rod 3 is located directly above the barrel 5, and can be inserted into the barrel 5 to press the titanium alloy raw material 6 in the barrel 5 into a titanium alloy integral electrode 8; the forming mold 7 is located directly below the barrel 5, and under the loading of the pressing rod 3, the titanium alloy integral electrode 8 is pressed and extruded downward from the mouth of the forming mold 7; the receiving device 9 is located directly below the forming mold 7, and is used to support the pressed titanium alloy integral electrode 8.
[0034] The lower plane position of the barrel 5 is the zero position of the upper surface position of the pressed electrode 8; the outlet position of the forming die 7 is the zero position of the length of the pressed electrode 8.
[0035] The PCL controller 11 collects the above data and integrates the cross-sectional areas of the barrel 5 and the forming die 7 input by the HMI human-machine interface 12 to calculate the density of the pressed titanium alloy electrode 8 in real time, and adjusts the holding time, the pressing speed of the pressing rod 3 and the end position of the pressing according to the density change.
[0036] Example 2
[0037] Based on Example 1, this embodiment provides a method for online detection and control of the overall forming density of a titanium alloy electrode. Figure 2 As shown, the following steps are included:
[0038] Step 1: Input the cross-sectional area S0 of the barrel 5 and the reference density ρ of the pressed integral electrode 8 to the PLC controller 11 through the HMI human-machine interface 12. 基准 .
[0039] Step 2: At the end of the previous cycle, before the pressing rod 3 rises and returns, the PLC controller 11 detects the position of the pressing rod 3 through the pressing rod displacement sensor 4 to obtain the upper surface position L of the entire electrode 8 in the previous cycle. 10 .
[0040] Step three, the pressing rod 3 rises and returns, the feeding device 1 is loaded, and the PLC controller 11 collects the weight m of the titanium alloy raw material in the feeding device 1 through the weighing sensor 2. The feeding device 1 enters above the barrel 5, pours all the titanium alloy raw material 6 into the barrel 5, and then returns to the outside of the barrel 5.
[0041] Step 4: The pressing rod 3 is lowered to press the whole electrode until the electrode 8 extruded from the forming die 6 pushes the receiving device 9 to move. When the displacement sensor 10 of the receiving device detects that the position of the pressed whole electrode 8 changes slightly, the PLC controller 11 obtains the position L of the upper surface of the electrode at this time through the pressing rod displacement sensor 4. 11 .
[0042] Step 5: The PLC controller 11 processes the data S0 and L obtained in the above steps. 10 ,m,L 11 Calculate and obtain the density ρ1 of the titanium alloy electrode pressed in this cycle, and compare it with the reference density ρ 基准 For comparison:
[0043] If ρ1<ρ 基准 , then, increase the holding time t of this pressing, increase the downward speed ν of the pressing rod 3, so as to increase the pressing force and thus increase the electrode density of this cycle pressing, and increase the stopping position L of this cycle pressing. 10 , in order to increase the pressing force of the next cycle and thus increase the electrode density of the next cycle pressing;
[0044] If ρ1>ρ 基准, then reduce the holding time t of this pressing, reduce the downward speed ν of the pressing rod 3, so as to reduce the pressing force and thus reduce the electrode density of this cycle pressing, and reduce the stopping position L of this cycle pressing. 10 , in order to reduce the pressing force in the next cycle and thus reduce the electrode density in the next cycle.
[0045] Step 6: The pressure rod 3 maintains the pressure for the time t, speed ν and stop position L as described in step 5. 10 After the pressure holding is completed, the whole electrode is pressed down continuously, and the electrode is extruded from the outlet of the forming die, pushing the receiving device to continue to move downward.
[0046] Step 7: Repeat the above cycle until the overall electrode 8 of the required length is obtained.
[0047] Wherein, the reference density ρ in step 1 基准 3.1~3.6g / cm 3 between;
[0048] The downward movement speed v of the press rod described in step five is between 1 and 10 mm / s.
[0049] Parts not specifically described in this embodiment belong to common knowledge and known techniques in the technical field and will not be described in detail here.
[0050] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A method for online detection and control of the overall forming density of a titanium alloy electrode, characterized in that: The titanium alloy electrode integral forming density online detection and control system is adopted, including the following steps: Step 1: Input the barrel cross-sectional area S0 and the reference density ρ of the pressed whole electrode into the PLC controller. 基准 ; Step 2: At the end of the last test or when the system starts working, before the press rod rises and returns, the PLC controller detects the position of the press rod through the press rod displacement sensor to obtain the overall electrode upper surface position L of the last test 10 ; Step 3: The pressing rod rises and returns, and the feeding device is loaded. The PLC controller collects the weight m of the titanium alloy raw material in the feeding device through the weighing sensor. The feeding device enters the top of the barrel and pours all the titanium alloy raw materials into the barrel and then returns to the outside of the barrel. Step 4: The press rod descends and presses the whole electrode until the electrode is squeezed out from the outlet of the forming die, pushing the receiving device to move. When the displacement sensor of the receiving device detects that the position of the whole electrode changes, the PLC controller obtains the position L of the upper surface of the electrode at this time through the press rod displacement sensor. 11 ; The PLC controller collects the data obtained by the step 2, and the data is the overall electrode upper surface position L 10 , the weight m of the titanium alloy raw material in the feeding device collected by the PLC controller through the weighing sensor in step 3 and the upper surface position L of the electrode obtained by the pressure rod displacement sensor in step 4 11 , and the density ρ1 of the pressed titanium alloy electrode is calculated in real time by combining the barrel cross-sectional area S0 and the forming die cross-sectional area input by the HMI human-machine interface; Step 5: Compare the density ρ1 of the pressed titanium alloy electrode with the reference density ρ 基准 For comparison: If ρ1<ρ 基准 , then increase the holding time t of this pressing, increase the downward speed ν of the pressing rod, and increase the stopping position L of this cycle pressing. 10 ; If ρ1>ρ 基准 , then reduce the holding time t of this pressing, reduce the downward speed ν of the pressing rod, and reduce the stopping position L of this cycle pressing 10 ; Step 6: The pressure rod maintains the pressure for the time t, speed ν and stop position L as described in step 5. 10 After the pressure is maintained, the whole electrode is pressed downwards, and the electrode is extruded from the outlet of the forming die, pushing the receiving device to continue to move downwards; Step 7, repeat steps 1 to 6 until the overall electrode of the required length is obtained; The online detection and control system for the overall forming density of the titanium alloy electrode comprises a barrel, a feeding device, a press rod, a receiving device, a weighing sensor, a press rod displacement sensor, a receiving device displacement sensor and an HMI human-machine interface, wherein the barrel is used to load the titanium alloy raw material; the feeding device is located outside the barrel and can enter above the barrel and add the titanium alloy raw material into the barrel; the weighing sensor is arranged on the feeding device and is used to measure the weight of the added titanium alloy raw material; the press rod is located directly above the barrel and can extend into the barrel to press the titanium alloy raw material in the barrel into a titanium alloy integral electrode, the press rod displacement sensor is arranged on the press rod, and the position of the lower surface of the pressed electrode is obtained by detecting the position of the press rod; a forming die is arranged directly below the barrel, the receiving device is located directly below the forming die, the receiving device displacement sensor is arranged on the receiving device, and the length of the pressed electrode is obtained by detecting the position of the receiving device, the weighing sensor, the press rod displacement sensor and the receiving device displacement sensor are all electrically connected to the PLC controller, and the HMI human-machine interface is electrically connected to the PLC controller.
2. The method for online detection and control of the overall forming density of titanium alloy electrodes according to claim 1 is characterized in that: The diameter of the forming die opening is smaller than the diameter of the barrel.
3. The method for online detection and control of the overall forming density of titanium alloy electrodes according to claim 1, characterized in that: The press rod is connected to the PLC controller by electrical signals, and the press rod can be adjusted by the PLC controller.
4. The method for online detection and control of the overall forming density of titanium alloy electrodes according to claim 1, characterized in that: Input the barrel cross-sectional area S0 and the reference density ρ of the pressed whole electrode to the PLC controller through the HMI human-machine interface 基准 .
Citation Information
Patent Citations
Method for measuring uniaxial compressibility of metal powder in warm-pressing state
CN113188948A
On-line automatic height measuring device for green anode
CN212270254U