A method for adsorbing cesium ions from high-salinity brine
The adsorbent prepared by transition metal salts and acids uses ion exchange and oxygen coordination technology to solve the problem of separation of low-concentration cesium ions in high-salt brine and achieve efficient and economical cesium ion adsorption.
Patent Information
- Application Number
- CN202310039296.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-12
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-01-12
AI Technical Summary
The existing technology has the problems of complex process, high cost, and poor selective adsorption when separating cesium ions from high-salt brine. In particular, it is difficult to achieve efficient adsorption in a low-concentration cesium ion environment.
The adsorbent is prepared by mixing transition metal salts and acids, and is prepared through hydrothermal reaction, filtration, washing and drying. It uses ion exchange and oxygen coordination to achieve selective adsorption of cesium ions, simplifying the process and reducing costs.
Efficient and selective adsorption of low-concentration cesium ions is achieved. The process is short and efficient, and the adsorbent preparation conditions are mild. It is suitable for the separation and extraction of cesium ions in high-salt brine.
Smart Images

Figure BDA0004050486210000101 
Figure BDA0004050486210000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of separation and recovery of valuable metals in brine, and relates to a method for adsorbing cesium ions, in particular to a method for adsorbing cesium ions from high-salt brine. Background Art
[0002] Cesium is located in Group IA of the sixth period. It is an alkali metal with a soft texture, ductility, and active properties. It is the most metallic element known and plays an important role in many fields such as medicine, electronic device manufacturing, and catalytic synthesis.
[0003] In nature, cesium mainly exists in ores and brines. Leaching cesium ions from ores causes serious environmental pollution, while extracting cesium resources from brine can avoid calcination and leaching, which is an environmentally friendly extraction method. In addition, cesium resources in brine are abundant. It is estimated that there are at least 6.17 million tons of cesium oxide in the Qarhan Salt Lake alone, but the concentration is low, less than 40 mg / L, and it often coexists with other alkali metal elements, such as lithium, sodium, potassium and calcium ions, with concentrations as high as 10-60 g / L, which is much higher than the cesium ion concentration, which brings high difficulty to the separation and purification of cesium. The current cesium ion separation technologies include chemical precipitation, solvent extraction and membrane separation.
[0004] CN106552602B discloses a preparation method of a composite adsorbent material for adsorbing rubidium and cesium ions, wherein a polymer layer containing a catechol structure is prepared by in-situ polymerization on the surface of a porous material, and then an ion exchange functional nano adsorbent layer is grown in-situ on the surface of the polymer layer to obtain a composite adsorbent material. The polymer layer containing a catechol structure on the surface of the porous material has a strong complex adsorption function of rubidium and cesium, and has a strong adhesion effect on the porous material and the ion exchange functional adsorbent, which greatly improves the stability of the composite adsorbent material, is conducive to the in-situ growth of the adsorbent, and the particle size of the adsorbent layer is adjustable and controllable; during adsorption, the solution is fully in contact with the adsorbent, and contacts with the polymer layer through the gap between the adsorbent particles, and rubidium and cesium are adsorbed by synergistic action, with a high adsorption capacity, which can be used for the adsorption of rubidium and cesium in salt lake brine and the adsorption of cesium in radioactive wastewater, but the technical solution cannot achieve the selective adsorption of rubidium and cesium, and further treatment is required for the separation of rubidium and cesium.
[0005] CN106435180A discloses a method for extracting rubidium ions and cesium ions, the method comprising extracting a mixed solution containing rubidium ions and cesium ions using a composite extractant, the composite extractant comprising an acidic extractant and at least one component of a neutral organic matter and a phenol extractant; the extraction method improves the extraction effect of rubidium ions and cesium ions. However, the extractant is not easy to synthesize, is expensive and easy to lose; an organic solvent is required, which is not environmentally friendly; strong acid or strong base needs to be added during the extraction process, and is not suitable for the separation and extraction of extremely low concentration cesium ions in salt lakes.
[0006] CN105363415B discloses a method for preparing a magnetic cesium ion adsorbent, comprising the steps of: coating amination silicon dioxide on the surface of ferroferric oxide to obtain coated ferroferric oxide; mixing a carboxylated crown ether derivative with a condensation agent to obtain a first mixture; placing the first mixture in a first solvent and stirring, then adding the coated ferroferric oxide, and reacting at 70-90° C. for 1-2 hours to obtain a second mixture; wherein the first solvent is used to dissolve the carboxylated crown ether derivative and the condensation agent; performing solid-liquid separation on the second mixture to obtain a first solid phase, washing and drying the first solid phase to obtain a magnetic cesium ion adsorbent, which has good cesium ion adsorption selectivity, can maintain stable adsorption performance in multiple adsorption-desorption cycles, and can be used to adsorb and separate cesium ions from systems such as radioactive nuclear waste, but the preparation process is complicated and the cost is high.
[0007] The invention provides a method for adsorbing cesium ions from high-salinity brine, which simplifies the process, reduces the cost, has high adsorption efficiency, and is suitable for selective adsorption of low-concentration cesium ions in high-salinity brine. Summary of the invention
[0008] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for adsorbing cesium ions from high-salinity brine, simplify the process, improve the adsorption efficiency and reduce the cost. The "high-salinity brine" mentioned in the present invention refers to brine with a concentration of other impurity metal ions ≥ 0.001 mol / L except cesium ions.
[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0010] The present invention provides a method for adsorbing cesium ions from high-salinity brine, the method comprising the following steps:
[0011] The high-salinity brine is mixed with the adsorbent to complete the adsorption of cesium ions;
[0012] The adsorbent is prepared by mixing a transition metal salt and an acid, and the resulting mixture is subjected to hydrothermal reaction, filtration, water washing and drying;
[0013] The concentration of cesium ions in the high-salinity brine is 0.2×10 -4 -1×10 -4 mol / L;
[0014] The pH of the mixture is 0.5-2.
[0015] The adsorbent prepared by using transition metal salt and acid as raw materials is used to adsorb cesium ions in high-salt brine. The cesium ions replace the cations in the adsorbent through ion exchange and carry out various coordination with a large amount of oxygen exposed inside the pores of the adsorbent, so that the cesium ions remain in the pores of the adsorbent. The adsorption capacity of the obtained adsorbent for other metal ions in the high-salt brine is far inferior to that of the cesium ions, thereby realizing the selective adsorption of low-concentration cesium ions. The method is short and efficient, the preparation conditions of the adsorbent are mild, and it is easy to promote.
[0016] The concentration of cesium ions in the high-salt brine of the present invention is 0.2×10 -4 -1×10 -4 mol / L, for example, 0.2×10 -4 mol / L、0.4×10 -4 mol / L、0.6×10 -4 mol / L、0.8×10 -4 mol / L or 1×10 -4 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0017] The pH of the mixture in the present invention is 0.5-2, for example, it can be 0.8, 1, 1.3, 1.5, 1.8 or 2, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable. The pH of the mixture is 0.5-2, which is conducive to obtaining an adsorbent with a high degree of molding and achieving the purpose of adsorbing cesium ions through ion exchange; when the pH>2, the adsorbent is not easy to mold, and the adsorption rate of cesium ions is reduced; when the pH<0.5, the demand for acid is high, but the adsorption of cesium ions does not change much, and the loss of acid is high.
[0018] Preferably, the concentration of the transition metal salt in the mixture is 1-3 mol / L, for example, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] The concentration of the transition metal salt in the mixture of the present invention is controlled within the range of 1-3 mol / L, and the obtained adsorbent has good molding degree and strong adsorption capacity for cesium ions; when the concentration of the transition metal salt in the mixture is lower than 1 mol / L, the adsorbent is not easy to be molded, and the adsorption capacity for cesium ions is weakened; when the concentration of the transition metal salt in the mixture is higher than 3 mol / L, the crystallinity of the obtained adsorbent may be affected, thereby reducing its adsorption capacity for cesium ions.
[0020] Preferably, the transition metal salt comprises any one or a combination of at least two of a molybdenum salt, a vanadium salt or a tungsten salt. Typical but non-limiting combinations include a combination of a molybdenum salt and a vanadium salt, a combination of a molybdenum salt and a tungsten salt, a combination of a vanadium salt and a tungsten salt, or a combination of a molybdenum salt, a vanadium salt and a tungsten salt.
[0021] Preferably, the molybdenum salt comprises any one of sodium molybdate dihydrate, sodium molybdate, ammonium molybdate or ammonium heptamolybdate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium molybdate dihydrate and sodium molybdate, a combination of sodium molybdate and ammonium molybdate, a combination of ammonium molybdate and ammonium heptamolybdate, a combination of sodium molybdate dihydrate, sodium molybdate and ammonium molybdate, or a combination of sodium molybdate dihydrate, sodium molybdate, ammonium molybdate and ammonium heptamolybdate.
[0022] Preferably, the vanadium salt comprises any one of sodium metavanadate, vanadium pentoxide or ammonium metavanadate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium metavanadate and vanadium pentoxide, a combination of vanadium pentoxide and ammonium metavanadate, a combination of sodium metavanadate and ammonium metavanadate, or a combination of sodium metavanadate, vanadium pentoxide and ammonium metavanadate.
[0023] Preferably, the tungsten salt includes any one of sodium tungstate dihydrate, sodium tungstate, ammonium tungstate or ammonium paratungstate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium tungstate dihydrate and sodium tungstate, a combination of sodium tungstate and ammonium tungstate, a combination of ammonium tungstate and ammonium paratungstate, or a combination of sodium tungstate dihydrate, sodium tungstate and ammonium tungstate.
[0024] Preferably, the acid comprises any one of concentrated nitric acid, concentrated sulfuric acid or concentrated hydrochloric acid, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of concentrated nitric acid and concentrated sulfuric acid, a combination of concentrated nitric acid and concentrated hydrochloric acid, a combination of concentrated sulfuric acid and concentrated hydrochloric acid, or a combination of concentrated nitric acid, concentrated sulfuric acid and concentrated hydrochloric acid.
[0025] Preferably, the high-salt brine comprises any one or a combination of at least two of sodium ions, potassium ions, magnesium ions, calcium ions or rubidium ions. Typical but non-limiting combinations include a combination of sodium ions and potassium ions, a combination of potassium ions and magnesium ions, a combination of magnesium ions and calcium ions, or a combination of calcium ions and rubidium ions.
[0026] Preferably, the concentration of sodium ions in the high-salt brine is 1-2.5 mol / L, for example, it can be 1 mol / L, 1.3 mol / L, 1.5 mol / L, 1.8 mol / L, 2 mol / L, 2.3 mol / L or 2.5 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the concentration of potassium ions in the high-salt brine is 1-2.5 mol / L, for example, it can be 1 mol / L, 1.3 mol / L, 1.5 mol / L, 1.8 mol / L, 2 mol / L, 2.3 mol / L or 2.5 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the concentration of magnesium ions in the high-salt brine is 1-2.5 mol / L, for example, it can be 1 mol / L, 1.3 mol / L, 1.5 mol / L, 1.8 mol / L, 2 mol / L, 2.3 mol / L or 2.5 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the concentration of calcium ions in the high-salt brine is 0.1×10 -2 -1×10 -2 mol / L, for example, 0.1×10 -2 mol / L、0.3×10 -2 mol / L、0.5×10 -2 mol / L、0.8×10 -2 mol / L or 1×10 -2 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the concentration of rubidium ions in the high-salinity brine is 0.1×10 -2 -1×10 -2 mol / L, for example, 0.1×10 -2 mol / L、0.3×10 -2 mol / L、0.5×10 -2 mol / L、0.8×10 -2 mol / L or 1×10 -2 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] Preferably, the transition metal salt and the acid are mixed with stirring at a rate of 200-600 rpm, for example, 200 rpm, 300 rpm, 400 rpm, 500 rpm or 600 rpm, but are not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0032] Preferably, the temperature of the hydrothermal reaction is 60-150°C, for example, it can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the hydrothermal reaction time is 0.5-6 h, for example, 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h or 6 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the drying temperature is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C, or 80°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] Preferably, the drying time is 6-24 h, for example, 6 h, 9 h, 12 h, 15 h, 18 h, 21 h or 24 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, the average particle size of the adsorbent is 1-5 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm or 5 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the one-dimensional ion channel size of the adsorbent is 0.55-0.6 nm, for example, 0.55 nm, 0.56 nm, 0.57 nm, 0.58 nm, 0.59 nm or 0.6 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] Preferably, the solid-liquid ratio of the adsorbent to the high-salt brine is (0.25-4):1, for example, it can be 0.25:1, 1:1, 2:1, 3:1 or 4:1, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable. The unit of the solid-liquid ratio is g / L.
[0039] Preferably, the temperature at which the high-salt brine is mixed with the adsorbent is 20-30°C, for example, 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] Preferably, the high-salt brine and the adsorbent are mixed for 1-6 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] Preferably, the high-salt brine is mixed with the adsorbent while being shaken, and the shaking rate is 100-300rpm, for example, 100rpm, 150rpm, 200rpm, 250rpm or 300rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0042] As a preferred technical solution of the method of the invention, the method comprises the following steps:
[0043] The high-salinity brine and the adsorbent are mixed at 20-30°C for 1-6 hours to complete the adsorption of cesium ions;
[0044] The solid-liquid ratio of the adsorbent to the high-salt brine during mixing is (0.25-4):1 g / L;
[0045] The concentration of cesium ions in the high-salinity brine is 0.2×10 -4 -1×10 -4 mol / L;
[0046] The adsorbent is prepared by mixing a transition metal salt and an acid, and the obtained mixture is subjected to a hydrothermal reaction at 60-150° C. for 0.5-6 h, filtered, washed with water and dried; the concentration of the transition metal salt in the mixture is 1-3 mol / L, and the transition metal salt includes any one of molybdenum salt, vanadium salt or tungsten salt or a combination of at least two thereof; the pH of the mixture is 0.5-2.
[0047] To achieve this object, the present invention adopts the following technical solutions:
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] The adsorbent prepared by using transition metal salt and acid as raw materials is used to adsorb cesium ions in high-salt brine. The cesium ions replace the cations in the adsorbent through ion exchange and carry out various coordination with a large amount of oxygen exposed in the pores of the adsorbent, so that the cesium ions remain in the pores of the adsorbent. The adsorption capacity of the obtained adsorbent for other metal ions in the high-salt brine is far inferior to that of the cesium ions, thereby realizing the selective adsorption of low-concentration cesium ions. The method is short and efficient, the preparation conditions of the adsorbent are mild, and it is easy to promote. DETAILED DESCRIPTION
[0050] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0051] Example 1
[0052] This embodiment provides a method for adsorbing cesium ions from high-salinity brine, the method comprising the following steps:
[0053] The concentration of cesium ions is 7.3×10 -5 mol / L high-salinity brine was mixed with the adsorbent at 25°C for 4 h, accompanied by shaking at a shaking rate of 200 rpm to complete the adsorption of cesium ions;
[0054] Wherein, the concentration of magnesium ions in the high-salt brine is 2 mol / L;
[0055] The solid-to-liquid ratio of the adsorbent to the high-salt brine during the mixing is 1:1 g / L;
[0056] The adsorbent is prepared by mixing a transition metal salt and concentrated nitric acid, and the resulting mixture is subjected to a hydrothermal reaction at 80° C. for 2 hours, filtered, washed with water, and dried at 70° C. for 18 hours; the concentration of the transition metal salt in the mixture is 1.5 mol / L, and the transition metal salt is sodium molybdate dihydrate; the pH of the mixture is 1.2;
[0057] The average pore size of the adsorbent is 3 μm, and the size of its one-dimensional ion channel is 0.58 nm.
[0058] Example 2
[0059] This embodiment provides a method for adsorbing cesium ions from high-salinity brine, the method comprising the following steps:
[0060] The concentration of cesium ions is 2.0×10 -5 mol / L high-salinity brine was mixed with the adsorbent at 20°C for 6 h, accompanied by shaking at a shaking rate of 300 rpm to complete the adsorption of cesium ions;
[0061] Wherein, the concentration of sodium ions in the high-salt brine is 2 mol / L;
[0062] The solid-liquid ratio of the adsorbent to the high-salt brine during the mixing is 0.25:1 g / L;
[0063] The adsorbent is prepared by mixing a transition metal salt and concentrated hydrochloric acid, and the resulting mixture is subjected to a hydrothermal reaction at 60° C. for 6 hours, filtered, washed with water, and dried at 60° C. for 24 hours; the concentration of the transition metal salt in the mixture is 1 mol / L, and the transition metal salt is sodium molybdate; the pH of the mixture is 2;
[0064] The average pore size of the adsorbent is 5 μm, and the size of its one-dimensional ion channel is 0.55 nm.
[0065] Example 3
[0066] This embodiment provides a method for adsorbing cesium ions from high-salinity brine, the method comprising the following steps:
[0067] The concentration of cesium ions is 1×10 -4 mol / L high-salinity brine was mixed with the adsorbent at 30°C for 1 h, accompanied by shaking at a shaking rate of 100 rpm to complete the adsorption of cesium ions;
[0068] Wherein, the concentration of potassium ions in the high-salt brine is 2 mol / L;
[0069] The solid-to-liquid ratio of the adsorbent to the high-salt brine during the mixing is 4:1 g / L;
[0070] The adsorbent is prepared by mixing a transition metal salt and concentrated sulfuric acid, and the resulting mixture is subjected to a hydrothermal reaction at 150° C. for 0.5 h, filtered, washed with water, and dried at 80° C. for 6 h; the concentration of the transition metal salt in the mixture is 3 mol / L, and the transition metal salt is ammonium molybdate; the pH of the mixture is 1;
[0071] The average pore size of the adsorbent is 1 μm, and the size of its one-dimensional ion channel is 0.6 nm.
[0072] Example 4
[0073] This embodiment provides a method for adsorbing cesium ions from high-salt brine. The method is the same as that of Embodiment 1 except that the concentration of the transition metal salt in the mixture is 0.5 mol / L.
[0074] Example 5
[0075] This embodiment provides a method for adsorbing cesium ions from high-salt brine. The method is the same as that of Embodiment 1 except that the concentration of the transition metal salt in the mixture is 4 mol / L.
[0076] Example 6
[0077] This embodiment provides a method for adsorbing cesium ions from high-salt brine. In the method, the concentration of magnesium ions in the high-salt brine is 4.2×10 -3 Except for mol / L, the rest are the same as in Example 1.
[0078] Example 7
[0079] This embodiment provides a method for adsorbing cesium ions from high-salt brine. In the method, the concentration of magnesium ions in the high-salt brine is 4.4×10 -2 Except for mol / L, the rest are the same as in Example 1.
[0080] Example 8
[0081] This embodiment provides a method for adsorbing cesium ions from high-salt brine. In the method, the concentration of magnesium ions in the high-salt brine is 1.9×10 -1 Except for mol / L, the rest are the same as in Example 1.
[0082] Example 9
[0083] This embodiment provides a method for adsorbing cesium ions from high-salinity brine, except that magnesium ions are replaced by calcium ions, and the concentration of calcium ions is 3.2×10 -3 Except for mol / L, the rest are the same as in Example 1.
[0084] Example 10
[0085] This embodiment provides a method for adsorbing cesium ions from high-salinity brine, except that magnesium ions are replaced by calcium ions, and the concentration of calcium ions is 2.6×10 -2 Except for the calcium ion of 1 mol / L, the rest is the same as that of Example 1.
[0086] Embodiment 11
[0087] This embodiment provides a method for adsorbing cesium ions from high-salinity brine, except that magnesium ions are replaced by calcium ions, and the concentration of calcium ions is 1.1×10 -1 Except for the calcium ion of 1 mol / L, the rest is the same as that of Example 1.
[0088] Comparative Example 1
[0089] This comparative example provides a method for adsorbing cesium ions from high-salinity brine, in which the method is the same as Example 1 except that the pH of the mixture is 0.25.
[0090] Comparative Example 2
[0091] This comparative example provides a method for adsorbing cesium ions from high-salinity brine. The method is the same as Example 1 except that the pH of the mixture is 3.
[0092] Performance Testing
[0093] According to the methods provided in Examples 1-11 and Comparative Examples 1 and 2, the contents of cesium ions and other metal ions in high-salt brine before and after adsorption were measured using an inductively coupled plasma optical emission spectrometer (ICP-OES), and the adsorption amount (mol / g) and adsorption rate (%) were calculated.
[0094] The results are shown in Table 1.
[0095] Table 1
[0096]
[0097]
[0098] As shown in Table 1, in the method provided by the present invention, the adsorption amount of cesium ions is 7.2×10 -5 mol / g, the adsorption rate is over 98%, while the adsorption rate of other metal ions in high-salt brine is only about 0.2%. The method has a much higher adsorption capacity for cesium ions than other metal ions in high-salt brine, and achieves selective adsorption of low-concentration cesium ions.
[0099] From the comparison between Example 4 and Example 5 and Example 1, it can be seen that when the concentration of the transition metal salt in the mixture of the present invention is controlled in the range of 1-3 mol / L, the obtained adsorbent has a strong adsorption capacity for cesium ions; when the concentration of the transition metal salt in the mixture is lower than 1 mol / L, the adsorbent is not easy to form, and the adsorption capacity for cesium ions is weakened. When the concentration of the transition metal salt is 0.5 mol / L, the adsorption amount of cesium ions by the obtained adsorbent is only 5.1×10 -5 mol / g, the adsorption capacity of the obtained adsorbent for cesium ions decreased; when the concentration of the transition metal salt in the mixture was higher than 3 mol / L, it would also affect the adsorption capacity of the obtained adsorbent for cesium ions. When the concentration of the transition metal salt was 4 mol / L, the adsorption capacity of the obtained adsorbent for cesium ions was 4.86×10 - 5 mol / g, and the adsorption rate was only 65.7%.
[0100] Examples 6-8 and Examples 9-11 respectively changed the concentrations of magnesium ions and calcium ions in the high-salt brine, but the adsorption rate of cesium ions by the adsorbent was in the range of 99.0-100%, which remained at a relatively high level. Therefore, changing the concentration of symbiotic ions in the high-salt brine will not affect the selective adsorption performance of cesium ions.
[0101] From the comparison of Comparative Examples 1 and 2 with Example 1, it can be seen that the pH of the mixture consisting of the transition metal salt and the acid is 0.5-2, which is conducive to obtaining an adsorbent with a high degree of molding; when the pH>2, the adsorbent is not easy to mold, which reduces the adsorption rate of cesium ions. When the pH is 3, the adsorption rate of cesium ions by the obtained adsorbent is only 83.3%; when the pH is <0.5, the demand for acid is high, but the adsorption of cesium ions does not change much, and the loss of acid is high. Therefore, the pH of the mixture needs to be controlled in the range of 1-2, which is conducive to ensuring that the selective adsorption of cesium ions in high-salt brine by the obtained adsorbent is at a high level.
[0102] In summary, the present invention provides a method for adsorbing cesium ions from high-salt brine. The adsorbent prepared by using transition metal salt and acid as raw materials is used to adsorb cesium ions in high-salt brine. The cesium ions replace the cations in the adsorbent through ion exchange, and carry out various coordination with a large amount of oxygen exposed inside the pores of the adsorbent, so that the cesium ions remain in the pores of the adsorbent. The adsorption capacity of the obtained adsorbent for other metal ions in the high-salt brine is far inferior to that of cesium ions, thereby achieving selective adsorption of low-concentration cesium ions. The method is short and efficient, with mild conditions and easy to promote.
[0103] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for adsorbing cesium ions from high-salinity brine, It is characterized in that The method comprises the following steps: The high-salinity brine is mixed with the adsorbent to complete the adsorption of cesium ions; The adsorbent is prepared by mixing a transition metal salt and an acid, and the resulting mixture is subjected to hydrothermal reaction, filtration, water washing and drying; The concentration of cesium ions in the high-salinity brine is 0.2×10 -4 -1×10 -4 mol / L; The pH of the mixture is 0.5-2; The transition metal salt includes a molybdenum salt, and the molybdenum salt includes any one of sodium molybdate dihydrate, sodium molybdate, ammonium molybdate or ammonium heptamolybdate, or a combination of at least two thereof.
2. The method according to claim 1, It is characterized in that The concentration of the transition metal salt in the mixture is 1-3 mol / L.
3. The method according to claim 1, It is characterized in that The transition metal salt also includes vanadium salt and / or tungsten salt.
4. The method according to claim 3, It is characterized in that The vanadium salt includes any one of sodium metavanadate, vanadium pentoxide or ammonium metavanadate, or a combination of at least two of them.
5. The method according to claim 3, It is characterized in that The tungsten salt includes any one of sodium tungstate dihydrate, sodium tungstate, ammonium tungstate or ammonium paratungstate, or a combination of at least two thereof.
6. The method according to claim 1, It is characterized in that The acid includes any one of concentrated nitric acid, concentrated sulfuric acid or concentrated hydrochloric acid, or a combination of at least two of them.
7. The method according to claim 1, It is characterized in that The high-salt brine includes any one of sodium ions, potassium ions, magnesium ions, calcium ions or rubidium ions, or a combination of at least two of them.
8. The method according to claim 7, It is characterized in that The concentration of sodium ions in the high-salt brine is 1-2.5 mol / L.
9. The method according to claim 7, It is characterized in that The concentration of potassium ions in the high-salt brine is 1-2.5 mol / L.
10. The method according to claim 7, It is characterized in that The concentration of magnesium ions in the high-salt brine is 1-2.5 mol / L.
11. The method according to claim 7, It is characterized in that The concentration of calcium ions in the high-salt brine is 0.1×10 -2 -1×10 -2 mol / L.
12. The method according to claim 7, It is characterized in that The concentration of rubidium ions in the high-salinity brine is 0.1×10 -2 -1×10 -2 mol / L.
13. The method according to claim 1, It is characterized in that The transition metal salt and the acid are mixed with stirring at a rate of 200-600 rpm.
14. The method according to claim 1, It is characterized in that The temperature of the hydrothermal reaction is 60-150°C.
15. The method according to claim 1, It is characterized in that The hydrothermal reaction time is 0.5-6h.
16. The method according to claim 1, It is characterized in that The drying temperature is 60-80°C.
17. The method according to claim 1, It is characterized in that The drying time is 6-24h.
18. The method according to claim 1, It is characterized in that The average particle size of the adsorbent is 1-5 μm.
19. The method according to claim 1, It is characterized in that The one-dimensional ion channel size of the adsorbent is 0.55-0.6 nm.
20. The method according to claim 1, It is characterized in that The solid-liquid ratio of the adsorbent to the high-salt brine is (0.25-4):1, and the unit of the solid-liquid ratio is g / L.
21. The method according to claim 1, It is characterized in that The temperature of the high-salinity brine and the adsorbent when mixed is 20-30°C.
22. The method according to claim 1, It is characterized in that The high-salt brine and the adsorbent are mixed for 1-6 hours.
23. The method according to claim 1, It is characterized in that The high-salinity brine and the adsorbent are mixed with shaking at a rate of 100-300 rpm.
24. The method according to claim 1, It is characterized in that The method comprises the following steps: The high-salinity brine and the adsorbent are mixed at 20-30°C for 1-6 hours to complete the adsorption of cesium ions; The solid-liquid ratio of the adsorbent to the high-salt brine during mixing is (0.25-4):1 g / L; The concentration of cesium ions in the high-salinity brine is 0.2×10 -4 -1×10 -4 mol / L; The adsorbent is prepared by mixing a transition metal salt and an acid, and the obtained mixture is subjected to a hydrothermal reaction at 60-150° C. for 0.5-6 h, filtered, washed with water and dried; the concentration of the transition metal salt in the mixture is 1-3 mol / L, and the transition metal salt includes any one of molybdenum salt, vanadium salt or tungsten salt or a combination of at least two thereof; the pH of the mixture is 0.5-2.