A high barrier packaging material and preparation method thereof
By using a barrier layer composed of polyethylene, ethylene-vinyl alcohol copolymer, lamellar nanomaterials and spherical alumina particles in aluminum-plastic packaging materials, combined with acetylated chitosan nanofibers, the existing technology solves the problem of oxygen and The problem of insufficient moisture barrier capability is achieved by achieving higher barrier effect and toughness.
Patent Information
- Application Number
- CN202310117221.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-15
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-02-15
AI Technical Summary
The oxygen and moisture barrier capabilities of existing aluminum-plastic packaging materials cannot meet the packaging requirements for medicine or precision equipment.
A barrier layer composed of polyethylene, ethylene-vinyl alcohol copolymer, lamellar nanomaterials, spherical alumina particles and acetylated chitosan nanofibers is used to prepare high-barrier packaging materials through a casting process to form a dense barrier layer. Improves gas and moisture barrier properties.
It significantly improves the oxygen and moisture barrier capabilities of packaging materials, extends the diffusion path of moisture, enhances toughness and tensile properties, and meets the packaging requirements of medicine and precision equipment.
Smart Images

Figure BDA0004078976110000061
Abstract
Description
Technical Field
[0001] The present application relates to the field of packaging materials, and in particular to a high barrier packaging material and a preparation method thereof. Background Art
[0002] The high barrier packaging material of the present application is an aluminum-plastic packaging material, which is a composite of aluminum foil and plastic. It has good mechanical properties such as stiffness, tensile strength, tear strength, and abrasion resistance, and has good barrier effects against ultraviolet light, oxygen, and moisture, so it is often used for precision packaging of precious items such as precision industrial equipment and medicines.
[0003] Existing aluminum-plastic packaging materials generally include an aluminum foil reflective layer on the surface, a PE film sealing layer on the inner layer, and a plastic woven cloth substrate on the middle layer. The PE film and the plastic woven cloth substrate are laminated by hot pressing, and the aluminum foil reflective layer and the plastic woven cloth substrate are laminated by adhesive. For the convenience of production, the adhesive is usually made of polyethylene material.
[0004] However, the oxygen and moisture barrier capabilities of polyethylene materials are still difficult to meet the packaging requirements for medicines or precision equipment. Summary of the invention
[0005] The present application provides a high-barrier packaging material and a preparation method thereof, which can effectively improve the barrier performance of aluminum-plastic packaging materials to oxygen and moisture, and meet the packaging requirements of medicines and precision equipment.
[0006] In a first aspect, the present application provides a high barrier packaging material, which comprises an aluminum foil, a PE adhesive layer, a barrier layer, a PE adhesive layer, a substrate and a PE film which are laminated in sequence, wherein the aluminum foil is laminated with a woven cloth through an adhesive layer, and the barrier layer comprises the following raw materials in parts by weight:
[0007] Polyethylene: 100 parts;
[0008] Ethylene-vinyl alcohol copolymer: 20-30 parts;
[0009] Sheet nanomaterials: 10-20 parts;
[0010] Spherical alumina particles: 5-10 parts;
[0011] Dispersing modifier: 1-3 parts;
[0012] Acetylated chitosan nanofibers: 10-20 parts.
[0013] In the above technical solution of the present application, the barrier layer substrate adopts polyethylene and ethylene-vinyl alcohol with high barrier properties, which can effectively improve the gas and moisture barrier properties of the adhesive layer and ensure the sealing performance. Furthermore, the present application adopts two forms of nanofillers, flaky nanomaterials and spherical alumina particles, to form a denser barrier layer, effectively extend the diffusion path of moisture, and improve the moisture barrier capacity. In addition, spherical alumina can also reduce friction resistance and promote the dispersion and cast extrusion of the adhesive layer.
[0014] Acetylated chitosan nanofibers are added in the present application, which can, on the one hand, play a toughening and strengthening effect, compensating for the decrease in toughness and tensile properties of the barrier layer caused by the addition of fillers; on the other hand, its fiber morphology can be combined with the aforementioned lamellar nanomaterials and spherical alumina particles to form a denser barrier layer, thereby improving the barrier effect against oxygen and moisture.
[0015] Furthermore, since chitosan nanofiber molecular chains contain more hydroxyl groups and have strong hydrophilicity, it is not conducive to improving the moisture barrier capacity of the adhesive layer. Therefore, the present application uses acetylated hydrophobically modified chitosan nanofibers to effectively overcome this problem.
[0016] It should be noted that the above-mentioned lamellar nanomaterials refer to carbon materials or silicate materials with a lamellar structure, such as graphite, graphene, montmorillonite, and bentonite.
[0017] Preferably, the substrate is PE woven fabric, PP woven fabric or PE and PP composite woven fabric.
[0018] Preferably, the PE adhesive layer is substantially a cast layer of PE material, and plays a bonding role through a cast (lamination) process.
[0019] Preferably, the D50 particle size of the spherical alumina particles is less than 500 nm, and more preferably the D50 particle size of the spherical alumina particles is 50 to 100 nm.
[0020] Preferably, the average length of the chitosan nanofibers is 30 nm to 50 nm.
[0021] Preferably, the acetylated chitosan nanofibers are obtained by reacting chitosan nanofibers, acetic anhydride and concentrated sulfuric acid in a mass ratio of 10:(4-6):(2-4).
[0022] In the acetylation modification, concentrated sulfuric acid can activate the hydroxyl groups of the chitosan nanofibers, causing an esterification reaction to obtain a sulfate intermediate, which is then replaced by acetic anhydride acyl groups to form acetate, completing the acetylation hydrophobic modification.
[0023] Preferably, the concentration of the concentrated sulfuric acid is 98wt%.
[0024] The preferred method for preparing the acetylated chitosan nanofibers is: dispersing the chitosan nanofibers in anhydrous acetic acid, adding concentrated sulfuric acid under heating and stirring conditions to carry out an esterification reaction; then adding acetic anhydride to carry out an acetylation reaction, filtering and separating the fibers after the reaction is completed, and washing with anhydrous ethanol to obtain the obtained fibers.
[0025] Preferably, the heating temperature is 50-60°C;
[0026] And / or, the esterification reaction time is 10 to 30 minutes;
[0027] And / or, the acetylation reaction time is 1 to 2 hours.
[0028] Preferably, the sheet nanomaterial is selected from one or more of montmorillonite, mica, kaolin, graphene, and graphene oxide.
[0029] Preferably, the particle size of the sheet nanomaterial is 100 to 500 nm, more preferably 100 to 300 nm.
[0030] Preferably, the dispersion modifier includes one or more of a long-chain alkyl silane coupling agent, a phenyl silane coupling agent, and an epoxy silane coupling agent.
[0031] Inorganic nanofillers with small particle size and high specific surface area have a tendency to agglomerate and precipitate in the system, making it difficult to disperse evenly. Therefore, adding appropriate hydrophobic silane coupling agents can promote the full dispersion of fillers and improve their water barrier capacity while ensuring the hydrophobicity of packaging materials.
[0032] Preferably, the dispersion modifier contains 20 to 30 wt % of trimethylmethoxysilane.
[0033] The ethylene-vinyl alcohol copolymer added in this application contains certain polar hydroxyl groups, which is not conducive to improving the compatibility with polyethylene and affects the performance of barrier properties; on the other hand, it will increase the permeability of moisture to the adhesive layer. For this reason, this application incorporates a small amount of trimethylmethoxysilane. In the raw material blending step before cast extrusion, its monomethoxy group can be hydrolyzed into silanol, so that it can react with the hydroxyl group of the ethylene-vinyl alcohol copolymer to reduce its polarity. More importantly, compared with silane coupling agents, it has a small molecular weight and high permeability. It can penetrate into the ethylene-vinyl alcohol copolymer molecules to fully consume hydroxyl groups and promote the improvement of the moisture barrier properties of the adhesive layer. Of course, the steric hindrance and dispersion effects of trimethylmethoxysilane are poor, and it is necessary to ensure the amount of the aforementioned silane coupling agent to promote the uniform distribution of nanofillers.
[0034] In the second aspect, the present application provides a method for preparing a high-barrier packaging material, which is characterized in that the steps are as follows: a barrier layer is obtained by extruding through a casting process, a PE adhesive layer is obtained by a casting process and spreads it on a substrate, and then the barrier layer and the substrate are compounded, and then a PE film is compounded on the side of the substrate away from the barrier layer through a casting process to obtain a composite sheet; a PE adhesive layer is obtained by a casting process and spreads it on the barrier layer surface of a composite sheet, and an aluminum foil is compounded with the composite sheet to obtain a high-barrier packaging material.
[0035] Preferably, in the casting process of the barrier layer, the temperature of the heating section is 180±5°C; the temperature of the plasticizing section is 220±5°C; and the temperature of the homogenizing section is 230±5°C.
[0036] The packaging material comprises, from outside to inside, aluminum foil, PE adhesive layer, barrier layer, PE adhesive layer, PE woven cloth and PE film. The PE woven cloth and PE film are made of the same material. The aluminum foil layer plays a reflective barrier role, and the PE film plays a sealing effect.
[0037] In summary, this application has the following beneficial effects:
[0038] 1. This application uses polyethylene and ethylene-vinyl alcohol copolymer as the base material, and uses flaky nanomaterials, spherical alumina particles and acetylated chitosan nanofibers as fillers. It can improve the barrier ability of the adhesive layer and packaging materials to oxygen and moisture while ensuring the tensile properties and tensile strength of the adhesive layer.
[0039] 2. The present application uses silane coupling agent and trimethylmethoxysilane as dispersing modifiers, which can promote the dispersion of fillers while improving the barrier ability of the adhesive layer to moisture. DETAILED DESCRIPTION
[0040] Preparation examples of raw materials and / or intermediates
[0041] Preparation Example 1: Acetylated chitosan nanofibers were prepared according to the following steps:
[0042] Disperse 1 kg of chitosan nanofibers (average length 30 nm) in 5 kg of anhydrous acetic acid, and add 0.3 kg of concentrated sulfuric acid dropwise while stirring in a 50°C water bath. Continue stirring for 20 min after the addition is complete to allow the esterification reaction to proceed. Then add 0.5 kg of acetic anhydride dropwise and stir for 1 h to allow the acetylation reaction to proceed. After the reaction is complete, filter and separate the fibers, and wash them three times with anhydrous ethanol.
[0043] Preparation Example 2: Acetylated chitosan nanofibers were prepared according to the following steps:
[0044] Disperse 1 kg of chitosan nanofibers (average length 30 nm) in 5 kg of anhydrous acetic acid, and add 0.4 kg of concentrated sulfuric acid dropwise while stirring in a 50°C water bath. Continue stirring for 10 min after the addition is complete to allow the esterification reaction to proceed. Then add 0.6 kg of acetic anhydride dropwise and stir for 1 h to allow the acetylation reaction to proceed. After the reaction is complete, filter and separate the fibers, and wash them three times with anhydrous ethanol.
[0045] Preparation Example 3, acetylated chitosan nanofibers were prepared according to the following steps:
[0046] Disperse 1 kg of chitosan nanofibers (average length 30 nm) in 5 kg of anhydrous acetic acid, and add 0.2 kg of concentrated sulfuric acid dropwise while stirring in a 50°C water bath. Continue stirring for 20 min after the addition is complete to allow the esterification reaction to proceed. Then add 0.4 kg of acetic anhydride dropwise and stir for 1 h to allow the acetylation reaction to proceed. After the reaction is complete, filter and separate the fibers, and wash them three times with anhydrous ethanol.
[0047] Example
[0048] Example 1, a high barrier packaging material, is prepared according to the following steps:
[0049] Step 1: Take 10 kg of polyethylene (LDPE, brand 2426H), 2 kg of ethylene-vinyl alcohol copolymer (ethylene molar content of 30%), 1.5 kg of nano-montmorillonite (D50 particle size of 200 nm), 0.5 kg of spherical alumina particles (D50 particle size of 100 nm), 0.3 kg of dispersion modifier (including 0.06 kg of trimethylmethoxysilane, 0.14 kg of hexadecyltrimethoxysilane), 1 kg of acetylated chitosan nanofibers obtained in Preparation Example 1, add them into a mixer and stir and mix, and after 1 hour, add the mixed raw materials into a casting machine for plasticization and melting. Among them, the temperature of the heating section is 180 ± 5 ° C; the temperature of the plasticization section is 215 ± 5 ° C; the temperature of the homogenization section is 225 ± 5 ° C; after plasticization, the barrier layer is cast.
[0050] Take LDPE (brand 1C7A, coating grade) as raw material, add it into the casting machine, cast it at 330±5℃ to obtain two-layer film, one layer is PE film, the other layer is PE adhesive layer, cast them on both sides of PE woven cloth (substrate), then compound the barrier layer obtained above on the PE adhesive layer, and cool it to obtain a composite sheet.
[0051] Step 2: Use LDPE (grade 1C7A) as raw material, add it into a casting machine, cast it at 330±5°C to obtain another PE adhesive layer, spread it on the barrier layer of the composite sheet, and fix the aluminum foil on the composite sheet through the PE adhesive layer to obtain a high barrier packaging material.
[0052] In the above-mentioned high barrier packaging material, the thickness of the aluminum foil is 6 μm, the thickness of the PE adhesive layer is 10 μm, the thickness of the barrier layer is 20 μm, the thickness of the base sheet is 1 mm, and the thickness of the PE film is 10 μm.
[0053] Example 2, a high barrier packaging material, is prepared according to the following steps:
[0054] Step 1: Take 10 kg of polyethylene (LDPE, brand 2426H), 2 kg of ethylene-vinyl alcohol copolymer (ethylene molar content of 30%), 1 kg of nano mica powder (D50 particle size of 200 nm), 1 kg of spherical alumina particles (D50 particle size of 100 nm), 0.4 kg of dispersion modifier (including 0.12 kg of trimethylmethoxysilane, 0.28 kg of hexadecyltrimethoxysilane), 1 kg of acetylated chitosan nanofibers obtained in Preparation Example 2, add them into a mixer and stir and mix, and after 1 hour, add the mixed raw materials into a casting machine for plasticization and melting. Among them, the temperature of the heating section is 190 ± 5 ° C; the temperature of the plasticizing section is 210 ± 5 ° C; the temperature of the homogenizing section is 225 ± 5 ° C; after plasticization, the barrier layer is cast.
[0055] Take LDPE (brand 1C7A, coating grade) as raw material, add it into the casting machine, cast it at 330±5℃ to obtain two-layer film, one layer is PE film, the other layer is PE adhesive layer, cast them on both sides of PE woven cloth (substrate), then compound the barrier layer obtained above on the PE adhesive layer, and cool it to obtain a composite sheet.
[0056] Step 2: Use LDPE (grade 1C7A) as raw material, add it into a casting machine, cast it at 330±5°C to obtain another PE adhesive layer, spread it on the barrier layer of the composite sheet, and fix the aluminum foil on the composite sheet through the PE adhesive layer to obtain a high barrier packaging material.
[0057] In the above-mentioned high barrier packaging material, the thickness of the aluminum foil is 6 μm, the thickness of the PE adhesive layer is 10 μm, the thickness of the barrier layer is 20 μm, the thickness of the base sheet is 1 mm, and the thickness of the PE film is 10 μm.
[0058] Example 3, a high barrier packaging material, is different from Example 1 in that the raw materials of the barrier layer are different, as follows:
[0059] Step 1: Take 10 kg of polyethylene (LDPE, brand 2426H), 3 kg of ethylene-vinyl alcohol copolymer (ethylene molar content of 30%), 1.5 kg of nano-montmorillonite (D50 particle size of 200 nm), 0.5 kg of spherical alumina particles (D50 particle size of 100 nm), 0.2 kg of dispersion modifier (including 0.05 kg of trimethylmethoxysilane, 0.15 kg of hexadecyltrimethoxysilane), 2 kg of acetylated chitosan nanofibers obtained in Preparation Example 3, add them into a mixer and stir and mix, and after 1 hour, add the mixed raw materials into a casting machine for plasticization and melting. Among them, the temperature of the heating section is 180 ± 5 ° C; the temperature of the plasticization section is 215 ± 5 ° C; the temperature of the homogenization section is 225 ± 5 ° C; after plasticization, the barrier layer is cast.
[0060] Example 4 is a high barrier packaging material, which is different from Example 1 in that an equal amount of a long-chain silane coupling agent is used in place of trimethylmethoxysilane in the dispersion modifier.
[0061] Example 5 is a high barrier packaging material, which is different from Example 1 in that an equal amount of trimethylmethoxysilane is used in the dispersion modifier to replace the long-chain silane coupling agent.
[0062] Comparative Example
[0063] Comparative Example 1 is a high barrier packaging material, which is different from Example 1 in that an equal amount of unmodified chitosan nanofibers is used to replace the acetylated chitosan nanofibers.
[0064] Comparative Example 2 is a high barrier packaging material, which differs from Example 1 in that an equal amount of nano-montmorillonite is used to replace the acetylated chitosan nanofibers.
[0065] Comparative Example 3 is a high barrier packaging material, which differs from Example 1 in that an equal amount of nano-montmorillonite is used to replace the spherical alumina particles.
[0066] Comparative Example 4 is a high barrier packaging material, which differs from Example 1 in that an equal amount of spherical alumina particles is used to replace the nano-montmorillonite.
[0067] Comparative Example 5 is a high barrier packaging material, which is different from Example 1 in that no flaky nanomaterials, spherical alumina particles and acetylated chitosan nanofibers are added to the barrier layer raw materials.
[0068] Performance testing
[0069] 1. Barrier performance: According to the provisions of GB / T 1038-2000, the barrier capacity of high barrier packaging materials to oxygen and water vapor is tested at 23°C and 50RH%.
[0070] 2. Tensile performance test: According to the provisions of GB / T 13022-1991, the tensile strength (MPa) and elongation at break (%) of the barrier layer are tested.
[0071] Table 1. Experimental results
[0072]
[0073] Result analysis:
[0074] (1) It can be seen from Examples 1 to 5 and Comparative Examples 1 to 5 and Table 1 that the present application can improve the barrier capacity of the packaging material of the present application to oxygen and moisture by adopting flaky nanomaterials, spherical alumina particles and acetylated chitosan nanofibers, and effectively compensate for the loss of tensile properties by acetylated chitosan nanofibers.
[0075] (2) Combining Example 1 and Examples 4 to 5 and Table 1, it can be seen that the present application uses a complex of trimethylmethoxysilane and a long-chain alkyl coupling agent and other hydrophobic coupling agents as a dispersing modifier, which can effectively reduce the oxygen and water vapor permeability of the packaging material. The reason may be that the long-chain alkyl coupling agent can adhere to the surface of the nano-sky and play a steric hindrance role through the long alkyl chain, inhibiting the agglomeration phenomenon, making the nano-filler dispersed evenly and giving full play to the barrier effect. However, trimethylmethoxysilane has no obvious steric hindrance and dispersing effects and good permeability. The hydrolyzed silanol can react with the hydroxyl group of the ethylene-vinyl alcohol copolymer to reduce its polarity, improve compatibility and barrier effect against moisture.
[0076] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high barrier packaging material, characterized in that: The invention comprises an aluminum foil, a PE adhesive layer, a barrier layer, a PE adhesive layer, a substrate and a PE film which are laminated in sequence. The aluminum foil is laminated with the woven fabric through the adhesive layer. The barrier layer comprises the following raw materials in parts by weight: Polyethylene: 100 parts; Ethylene-vinyl alcohol copolymer: 20-30 parts; Sheet nanomaterial: 10-20 parts; Spherical alumina particles: 5-10 parts; Dispersing modifier: 1 to 5 parts; Acetylated chitosan nanofiber: 10-20 parts; The substrate is PE woven fabric, PP woven fabric or PE and PP composite woven fabric; The dispersion modifier is trimethylmethoxysilane or hexadecyltrimethoxysilane, and the dispersion modifier contains 20 to 30 wt% of trimethylmethoxysilane; The acetylated chitosan nanofibers are obtained by reacting chitosan nanofibers, acetic anhydride and concentrated sulfuric acid in a mass ratio of 10:(4-6):(2-4); The preparation method of the acetylated chitosan nanofibers comprises: dispersing the chitosan nanofibers in anhydrous acetic acid, adding concentrated sulfuric acid dropwise under heating and stirring conditions to carry out an esterification reaction; then adding acetic anhydride dropwise to carry out an acetylation reaction, filtering and separating the fibers after the reaction is completed, and washing with anhydrous ethanol to obtain the obtained fibers; The heating temperature is 50-60°C; And / or, the esterification reaction time is 10 to 30 minutes; And / or, the acetylation reaction time is 1 to 2 hours.
2. The high barrier packaging material according to claim 1, characterized in that: The sheet nanomaterial is selected from one or more of montmorillonite, mica, kaolin, graphene, and graphene oxide.
3. The method for preparing a high barrier packaging material according to any one of claims 1 to 2, characterized in that: Here are the steps: The barrier layer is extruded by a casting process, the PE adhesive layer is obtained by a casting process and spread on the substrate, and then the barrier layer and the substrate are composited, and then the PE film is composited on the side of the substrate away from the barrier layer by a casting process to obtain a composite sheet; A PE adhesive layer is obtained through a casting process and spread on the surface of the barrier layer of a composite sheet. The aluminum foil is compounded with the composite sheet to obtain a high-barrier packaging material.
Citation Information
Cited By
Composite aluminum foil packaging material and preparation method thereof
CN120942744A
Composite aluminum foil packaging material and method for manufacturing the same
CN120942744B