Method for preparing glass ceramic restoration and glass ceramic restoration prepared by using the same

By using lithium phosphate as a nucleation agent in the preparation process of lithium disilicate glass ceramics, the water absorption of phosphorus pentoxide and the decomposition of ammonium dihydrogen phosphate are avoided, the problem of unstable product performance is solved, and high strength is achieved and high crystallinity ceramic restoration.

CN116081926BActive Publication Date: 2024-12-03ZIRDENT NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211627301.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-12-03
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

During the preparation of lithium disilicate glass ceramics, the traditional nucleation agent phosphorus pentoxide is prone to absorb water and agglomeration, resulting in waste of mass and unstable performance. The decomposition of ammonium dihydrogen phosphate produces gas and loss, affecting product performance.

Method used

Lithium phosphate is used as the nucleation agent. By first preparing the basic glass powder, then mixing it with lithium phosphate and colorant for compression molding and sintering, the sublimation and loss of lithium phosphate are avoided, and the stability of the component and nucleation ability are ensured.

Benefits of technology

It effectively avoids the sublimation and loss of lithium phosphate, improves the mechanical properties and stability of the product, ensures the crystallinity and strength of lithium disilicate, and meets clinical requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004004088980000061
    Figure BDA0004004088980000061
  • Figure BDA0004004088980000071
    Figure BDA0004004088980000071
  • Figure BDA0004004088980000131
    Figure BDA0004004088980000131
Patent Text Reader

Abstract

The present application relates to a glass ceramic restoration and a preparation method thereof. The preparation method comprises the following steps: first preparing a basic glass powder, then mixing the basic glass powder, lithium phosphate and a colorant, and sequentially performing the steps of pressing, sintering and porcelain baking. On the one hand, the content of each component can be accurately controlled, and on the other hand, the lithium phosphate can be avoided from being wasted due to the high temperature of melting when it is added during the preparation of the basic glass powder. Moreover, the density of the green body after pressing has reached more than 70%, and the subsequent sintering heating rate can be set faster, further avoiding the sublimation of lithium phosphate, retaining more nucleation components, and ensuring the stability and nucleation ability of the original components, thereby effectively improving the performance and stability of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass ceramics, and in particular to a method for preparing a glass ceramic restoration and a glass ceramic restoration prepared by the method. Background Art

[0002] With the rapid development of science and technology in various countries, people's quality of life has gradually improved, and the cost of investment in themselves has also gradually increased. Teeth, as an important organ of the human body, are indispensable in people's lives. With the gradual aging of the population in China, the demand for teeth is particularly important. As a new type of dental material, lithium disilicate glass ceramics have excellent mechanical and physical and chemical properties from a professional perspective, and are safe and non-toxic; from an aesthetic perspective, they have good transparency and a color closer to natural teeth.

[0003] In the preparation process of lithium disilicate glass ceramics, a nucleating agent is usually added to form lithium disilicate crystals. The traditional nucleating agent is phosphorus pentoxide, which will synthesize lithium phosphate with lithium oxide, and a trace amount of nano-scale lithium phosphate crystal nuclei will become the nucleation particles of lithium metasilicate and lithium disilicate. However, due to the enhanced water absorption capacity of phosphorus pentoxide, direct mixing is easy to agglomerate, and in many cases it is added in the form of ammonium dihydrogen phosphate. Ammonium dihydrogen phosphate decomposes into phosphorus pentoxide, water and ammonia at about 300°C. Among them, 100g of ammonium dihydrogen phosphate will decompose at about 300°C to produce about 23.5g of water vapor and 14.8g of ammonia, and the remaining solid that neither burns nor supports combustion - phosphorus pentoxide is about 61.7g. It can be seen that this form of addition produces a lot of mass waste during preparation. At the same time, the boiling point of phosphorus pentoxide is only 360°C, while the subsequent melting temperature of glass ceramics is above 1200°C, and the subsequent sintering or die-casting is also carried out at 800°C to 900°C or higher, which will cause a large amount of phosphorus pentoxide to be lost. Therefore, the amount of ammonium dihydrogen phosphate added with a content of 3wt.% to 7wt.% is actually very small, and the lost quality cannot be accurately controlled, resulting in unstable product performance. If the phosphorus pentoxide required for the experiment is lost too much during the reaction process, lithium disilicate will not be able to effectively nucleate, which will have a great impact on the various aspects of the performance of the prepared lithium disilicate, and the mechanical properties of the product will not meet clinical requirements.

[0004] Since the key to the nucleation of lithium disilicate lies in the particles of lithium phosphate, directly adding lithium phosphate is a feasible method. However, the boiling point of lithium phosphate is only 158°C under standard atmospheric pressure, and it also has problems such as easy sublimation and corrosion. Summary of the invention

[0005] Based on this, it is necessary to provide a method for preparing glass-ceramic restorations that can effectively avoid the sublimation of lithium phosphate, retain more nucleation components, ensure the stability and nucleation ability of the original components, and thereby improve product performance and stability.

[0006] A method for preparing a glass ceramic restoration comprises the following steps:

[0007] Providing preparation raw materials, the preparation raw materials comprising basic glass powder raw materials, lithium phosphate and colorant;

[0008] After the basic glass powder raw materials are uniformly mixed, they are sequentially melted, water quenched, dried, and ground to obtain the basic glass powder;

[0009] The basic glass powder, lithium phosphate and colorant are mixed evenly, and then pressed into a shape to obtain a green body;

[0010] The green body is sintered and then porcelain fired to obtain the glass ceramic restoration.

[0011] The preparation method of the above-mentioned glass-ceramic restoration first prepares a basic glass powder, and then mixes the basic glass powder, lithium phosphate and a colorant to carry out the steps of pressing, sintering and porcelain baking in sequence. On the one hand, the content of each component can be accurately controlled, and on the other hand, the lithium phosphate can be avoided from being wasted due to the high melting temperature during the preparation of the basic glass powder. The density of the green body after pressing has reached more than 70%, and the subsequent sintering heating rate can be set faster, which further avoids the sublimation of lithium phosphate, retains more nucleation components, and ensures the stability and nucleation ability of the original components, thereby effectively improving the performance and stability of the product.

[0012] In one embodiment, the basic glass powder raw materials include silicon dioxide, lithium oxide, potassium oxide, aluminum oxide, zinc oxide and zirconium oxide.

[0013] In one embodiment, the colorant includes cerium oxide, vanadium pentoxide, erbium oxide and ferrosoferric oxide.

[0014] In one of the embodiments, the preparation raw materials include, by mass percentage, 0.1% to 2% lithium phosphate, 50% to 80% silicon dioxide, 10% to 25% lithium oxide, 2% to 8% potassium oxide, 1% to 6% aluminum oxide, 1% to 4% zinc oxide, 0 to 6% zirconium oxide, 0.5% to 3% cerium oxide, 0.1% to 1% vanadium pentoxide, 0.5% to 3% erbium oxide and 0 to 0.5% ferrosoferric oxide.

[0015] In one embodiment, the melting temperature is 1400°C to 1500°C.

[0016] In one embodiment, before the basic glass powder, lithium phosphate and colorant are mixed evenly, the step of dissolving the lithium phosphate in a solvent and then drying is also included.

[0017] In one embodiment, the pressing molding is dry pressing molding or hot isostatic pressing molding, the pressure of the dry pressing molding is 10MPa to 80MPa, the temperature of the hot isostatic pressing molding is 950℃ to 980℃, and the pressure is 10MPa to 40MPa.

[0018] In one of the embodiments, the sintering is performed under vacuum conditions, the sintering temperature is 700° C. to 800° C., and the heating rate is 5° C. / min to 10° C. / min.

[0019] In one of the embodiments, the temperature of the porcelain is 800°C to 900°C, the heating rate is 5°C / min to 10°C / min, and the holding time is 2min to 30min.

[0020] In addition, the present application also provides a glass ceramic restoration made using any of the above-mentioned preparation methods.

[0021] The glass ceramic restoration prepared by the above method can reach a strength of 350MPa-550MPa, a crystallinity of 70%-90%, and a fracture toughness of 2.4MPa·m 1 / 2 . DETAILED DESCRIPTION

[0022] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are provided. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0024] A method for preparing a glass ceramic restoration according to one embodiment includes the following steps S110 to S140:

[0025] S110, providing preparation raw materials.

[0026] Among them, the preparation raw materials include basic glass powder raw materials, lithium phosphate (Li3PO4) and colorants.

[0027] Furthermore, the basic glass powder raw materials include silicon dioxide (SiO2), lithium oxide (Li2O), potassium oxide (K2O), aluminum oxide (Al2O3), zinc oxide (ZnO) and zirconium oxide (ZrO2).

[0028] It will be appreciated that the above oxides can be obtained using their corresponding carbonates or nitrates.

[0029] Further, the colorant includes cerium oxide (CeO2), vanadium pentoxide (V2O5), erbium oxide (Er2O3) and ferrosoferric oxide (Fe3O4).

[0030] Furthermore, taking the total mass content of the raw materials as 100%, the raw materials include 0.1% to 2% Li3PO4, 50% to 80% SiO2, 10% to 25% Li2O, 2% to 8% K2O, 1% to 6% Al2O3, 1% to 4% ZnO, 0 to 6% ZrO2, 0.5% to 3% CeO2, 0.1% to 1% V2O5, 0.5% to 3% Er2O3 and 0 to 0.5% Fe3O4.

[0031] S120, after uniformly mixing the above-mentioned basic glass powder raw materials, sequentially melting, water quenching, drying and grinding are performed to obtain basic glass powder.

[0032] The melting temperature is 1400°C to 1500°C.

[0033] The average particle size of the base glass powder after grinding is 10 μm to 50 μm.

[0034] S130, after uniformly mixing the above-mentioned basic glass powder, lithium phosphate and colorant, pressing and molding to obtain a green body.

[0035] In this embodiment, before the basic glass powder, lithium phosphate and colorant are uniformly mixed, the step of dissolving the lithium phosphate in a solvent (such as ammonia water, water, dilute acid) and then drying is also included.

[0036] Lithium phosphate is dissolved in a solvent and then dried, and then mixed with basic glass powder and colorant. This can not only achieve precise composition control, but also avoid the waste of lithium phosphate sublimation due to the high melting temperature.

[0037] Furthermore, the pressing is dry pressing or hot isostatic pressing, wherein the pressure of dry pressing is 10 MPa to 80 MPa, and the temperature of hot isostatic pressing is 950° C. to 980° C. and the pressure is 10 MPa to 40 MPa.

[0038] S140, sintering the green body and then performing porcelain firing to obtain a glass ceramic restoration.

[0039] In this embodiment, the sintering is performed under vacuum conditions, the sintering temperature is 700° C. to 800° C., and the heating rate is 5° C. / min to 10° C. / min.

[0040] The semi-finished product obtained after sintering is purple and has a crystallinity of 30% to 50%.

[0041] The temperature of the porcelain is 800℃~900℃, the heating rate is 5℃ / min~10℃ / min, and the holding time is 2min~30min.

[0042] The setting of through-hole porcelain conditions can make the color of glass-ceramic restorations close to the color of real teeth.

[0043] In the above-mentioned preparation method of glass-ceramic restoration, since lithium phosphate itself is very stable and has a melting point of about 1300°C, lithium phosphate is used as a nucleating agent and directly mixed with the basic glass powder and the colorant, and then pressed, sintered and baked in sequence, which can effectively avoid its decomposition and sublimation during the preparation process. It can be used as an effective nucleating agent for the crystallization of lithium disilicate, which not only saves production costs but also facilitates composition control. The final ceramic restoration has controllable crystal morphology and excellent mechanical properties.

[0044] The glass ceramic restoration prepared by the above method has an average crystal size of 6nm to 35nm, and the morphology of the single crystal phase equiaxed lithium disilicate crystals is a rod-like structure with a diameter of 0.8μm to 1μm and a length of 2μm to 10μm. The strength of the glass ceramic restoration is 350MPa to 550MPa, the crystallinity reaches 70% to 90%, the phosphorus content is 0.025wt.% to 0.55wt.%, and the fracture toughness is 2.4MPa·m 1 / 2 .

[0045] The following are specific embodiments

[0046] The raw material compositions of lithium disilicate glass ceramics prepared in the following examples and comparative examples are shown in Table 1, wherein the content of each component is expressed in mass percentage.

[0047] It should be noted that each oxide in Table 1 can be obtained using its corresponding carbonate, oxide or nitrate.

[0048] Table 1

[0049]

[0050]

[0051] Comparative Example 1

[0052] This comparative example provides a lithium disilicate glass ceramic, and the preparation method of the lithium disilicate glass ceramic is as follows:

[0053] a. Weigh each matrix raw material according to the mass of each component of the comparative example in Table 1, and then pour the matrix raw materials into a ball mill for mixing to ensure that the basic glass powder is evenly mixed;

[0054] b. Put the evenly mixed basic glass powder into a crucible, heat it to 1450°C in a sintering furnace at a heating rate of 10°C / min, and keep it warm for 1 hour to obtain a basic glass liquid;

[0055] c. quenching the prepared basic glass liquid with water to obtain a glass frit;

[0056] d. After drying the obtained glass frit, put it into a ball mill for grinding to form a basic glass powder with an average particle size of 10 to 50 μm;

[0057] e. Processing the obtained basic glass powder into green ceramic blocks by dry pressing or isostatic pressing;

[0058] f. The green ceramic block is heated to 700°C at a heating rate of 10°C / min and sintered in vacuum for 1 hour, after which the glass body is cooled in the furnace. The main component of the glass body obtained at this time is lithium disilicate, and the color of the semi-finished product is purple;

[0059] g. Finally, the semi-finished product is cut and placed in a porcelain furnace at a heating rate of 10°C / min. The temperature is raised to 880°C and kept at that temperature for 30 minutes. The finished product is then cooled in the furnace and the sintered product has a color close to that of real teeth.

[0060] After testing, the product prepared in Comparative Example 1 has a strength of 372 MPa, a crystallinity of 72.5%, and a phosphorus content of 0.03%.

[0061] Example 1

[0062] This embodiment provides a low-phosphorus added glass ceramic restoration, the preparation method of which is as follows:

[0063] a. Pour the basic glass powder raw materials of Example 1 in Table 1 into a ball mill for mixing to ensure that the basic glass powder raw materials are mixed evenly;

[0064] b. Put the mixed glass powder raw materials into a crucible, heat them to 1450°C at a heating rate of 10°C / min in a sintering furnace, and keep them warm for 1 hour to obtain a basic glass liquid;

[0065] c. quenching the prepared basic glass liquid with water to obtain a glass frit;

[0066] d. After drying the obtained glass frit, put it into a ball mill for grinding to form a basic glass powder with an average particle size of 10 μm to 50 μm;

[0067] e. Mixing the above-mentioned basic glass powder, colorant and lithium phosphate, wherein the lithium phosphate is added by dissolving it in ammonia water and then drying it, and pressing and molding after mixing to obtain a green body;

[0068] f. The green body is heated to 700°C at a heating rate of 10°C / min and sintered in vacuum for 1 hour, after which the glass body is cooled in the furnace. The main component of the glass body obtained at this time is lithium disilicate, and the color of the semi-finished product is purple;

[0069] g. Finally, the semi-finished product is cut and placed in a porcelain furnace at a heating rate of 10°C / min. The temperature is raised to 880°C and kept at that temperature for 30 minutes. The finished product is then cooled in the furnace and the sintered product has a color close to that of real teeth.

[0070] After testing, the product prepared in Example 1 has a strength of 350 MPa, a crystallinity of 70.9%, and a phosphorus content of 0.025%.

[0071] Example 2

[0072] This embodiment provides a low-phosphorus added glass ceramic restoration, the preparation method of which is as follows:

[0073] a. Pour the basic glass powder raw materials of Example 2 in Table 1 into a ball mill for mixing to ensure that the basic glass powder raw materials are evenly mixed;

[0074] b. Put the evenly mixed basic glass powder raw materials into a crucible, heat them to 1450° C. at a heating rate of 10° C. / min in a sintering furnace, and keep them warm for 1 hour to obtain basic glass liquid;

[0075] c. quenching the prepared basic glass liquid with water to obtain a glass frit;

[0076] d. After drying the obtained glass frit, put it into a ball mill for grinding to form a basic glass powder with an average particle size of 10 μm to 50 μm;

[0077] e. Mixing the above-mentioned basic glass powder, colorant and lithium phosphate, wherein the lithium phosphate is added by dissolving it in ammonia water and then drying it, and then pressing and molding it to obtain a green body;

[0078] f. The green body is heated to 700°C at a heating rate of 10°C / min and sintered in vacuum for 1 hour, after which the glass body is cooled in the furnace. The main component of the glass body obtained at this time is lithium disilicate, and the color of the semi-finished product is purple;

[0079] g. Finally, the semi-finished product is cut and placed in a porcelain furnace at a heating rate of 10°C / min. The temperature is raised to 880°C and kept at that temperature for 30 minutes. The finished product is then cooled in the furnace and the sintered product has a color close to that of real teeth.

[0080] After testing, the product prepared in Example 2 has a strength of 376 MPa, a crystallinity of 73.7%, and a phosphorus content of 0.11%.

[0081] Example 3

[0082] This embodiment provides a low-phosphorus added glass ceramic restoration, the preparation method of which is as follows:

[0083] a. Pour the basic glass powder raw materials of Example 3 in Table 1 into a ball mill for mixing to ensure that the basic glass powder raw materials are mixed evenly;

[0084] b. Put the evenly mixed basic glass powder raw materials into a crucible, heat them to 1450° C. at a heating rate of 10° C. / min in a sintering furnace, and keep them warm for 1 hour to obtain basic glass liquid;

[0085] c. quenching the prepared basic glass liquid with water to obtain a glass frit;

[0086] d. After drying the obtained glass frit, put it into a ball mill for grinding to form a basic glass powder with an average particle size of 10 μm to 50 μm;

[0087] e. Mixing the above-mentioned basic glass powder, colorant and lithium phosphate, wherein the lithium phosphate is added by dissolving it in ammonia water and then drying it, and then pressing and molding it to obtain a green body;

[0088] f. The green body is heated to 700°C at a heating rate of 10°C / min and sintered in vacuum for 1 hour, after which the glass body is cooled in the furnace. The main component of the glass body obtained at this time is lithium disilicate, and the color of the semi-finished product is purple;

[0089] g. Finally, the semi-finished product is cut and placed in a porcelain furnace at a heating rate of 10°C / min. The temperature is raised to 880°C and kept at that temperature for 30 minutes. The finished product is then cooled in the furnace and the sintered product has a color close to that of real teeth.

[0090] After testing, the product prepared in Example 3 has a strength of 396 MPa, a crystallinity of 76.8%, and a phosphorus content of 0.2%.

[0091] Example 4

[0092] This embodiment provides a low-phosphorus added glass ceramic restoration, the preparation method of which is as follows:

[0093] a. Pour the basic glass powder raw materials of Example 4 in Table 1 into a ball mill for mixing to ensure that the basic glass powder raw materials are evenly mixed;

[0094] b. Put the evenly mixed basic glass powder raw materials into a crucible, heat them to 1450° C. at a heating rate of 10° C. / min in a sintering furnace, and keep them warm for 1 hour to obtain basic glass liquid;

[0095] c. quenching the prepared basic glass liquid with water to obtain a glass frit;

[0096] d. After drying the obtained glass frit, put it into a ball mill for grinding to form a basic glass powder with an average particle size of 10 μm to 50 μm;

[0097] e. Mixing the above-mentioned basic glass powder, colorant and lithium phosphate, wherein the lithium phosphate is added by dissolving it in ammonia water and then drying it, and then pressing and molding it to obtain a green body;

[0098] f. The green body is heated to 700°C at a heating rate of 10°C / min and sintered in vacuum for 1 hour, after which the glass body is cooled in the furnace. The main component of the glass body obtained at this time is lithium disilicate, and the color of the semi-finished product is purple;

[0099] g. Finally, the semi-finished product is cut and placed in a porcelain furnace at a heating rate of 10°C / min. The temperature is raised to 880°C and kept at that temperature for 30 minutes. The finished product is then cooled in the furnace and the sintered product has a color close to that of real teeth.

[0100] After testing, the product prepared in Example 4 has a strength of 433 MPa, a crystallinity of 79.6%, and a phosphorus content of 0.29%.

[0101] Example 5

[0102] This embodiment provides a low-phosphorus added glass ceramic restoration, the preparation method of which is as follows:

[0103] a. Pour the basic glass powder raw materials of Example 5 in Table 1 into a ball mill for mixing to ensure that the basic glass powder raw materials are mixed evenly;

[0104] b. Put the evenly mixed basic glass powder raw materials into a crucible, heat them to 1450° C. at a heating rate of 10° C. / min in a sintering furnace, and keep them warm for 1 hour to obtain basic glass liquid;

[0105] c. quenching the prepared basic glass liquid with water to obtain a glass frit;

[0106] d. After drying the obtained glass frit, put it into a ball mill for grinding to form a basic glass powder with an average particle size of 10 μm to 50 μm;

[0107] e. Mixing the prepared basic glass powder, colorant and lithium phosphate, wherein the lithium phosphate is added by dissolving it in ammonia water and then drying it, and then pressing and molding the mixed material to obtain a green body;

[0108] f. The green body is heated to 700°C at a heating rate of 10°C / min and sintered in vacuum for 1 hour, after which the glass body is cooled in the furnace. The main component of the glass body obtained at this time is lithium disilicate, and the color of the semi-finished product is purple;

[0109] g. Finally, the semi-finished product is cut and placed in a porcelain furnace at a heating rate of 10°C / min. The temperature is raised to 880°C and kept at that temperature for 30 minutes. The finished product is then cooled in the furnace and the sintered product has a color close to that of real teeth.

[0110] After testing, the product prepared in Example 5 has a strength of 487 MPa, a crystallinity of 82.5%, and a phosphorus content of 0.38%.

[0111] Example 6

[0112] This embodiment provides a low-phosphorus added glass ceramic restoration, the preparation method of which is as follows:

[0113] a. Pour the basic glass powder raw materials of Example 6 in Table 1 into a ball mill for mixing to ensure that the basic glass powder raw materials are mixed evenly;

[0114] b. Put the evenly mixed basic glass powder raw materials into a crucible, heat them to 1450° C. at a heating rate of 10° C. / min in a sintering furnace, and keep them warm for 1 hour to obtain basic glass liquid;

[0115] c. quenching the prepared basic glass liquid with water to obtain a glass frit;

[0116] d. After drying the obtained glass frit, put it into a ball mill for grinding to form a basic glass powder with an average particle size of 10 μm to 50 μm;

[0117] e. Mixing the above-mentioned basic glass powder, colorant and lithium phosphate, wherein the lithium phosphate is added by dissolving in cold water and then drying, and then pressing and molding after mixing to obtain a green body;

[0118] f. The green body is heated to 700°C at a heating rate of 10°C / min and sintered in vacuum for 1 hour, after which the glass body is cooled in the furnace. The main component of the glass body obtained at this time is lithium disilicate, and the color of the semi-finished product is purple;

[0119] g. Finally, the semi-finished product is cut and placed in a porcelain furnace at a heating rate of 10°C / min. The temperature is raised to 880°C and kept at that temperature for 30 minutes. The finished product is then cooled in the furnace and the sintered product has a color close to that of real teeth.

[0120] After testing, the product has a strength of 365MPa, a crystallinity of 73.2%, and a phosphorus content of 0.08%.

[0121] Example 7

[0122] This embodiment provides a low-phosphorus added glass ceramic restoration, the preparation method of which is as follows:

[0123] a. Pour the basic glass powder raw materials of Example 7 in Table 1 into a ball mill for mixing to ensure that the basic glass powder raw materials are mixed evenly;

[0124] b. Put the evenly mixed basic glass powder raw materials into a crucible, heat them to 1450° C. at a heating rate of 10° C. / min in a sintering furnace, and keep them warm for 1 hour to obtain basic glass liquid;

[0125] c. quenching the prepared basic glass liquid with water to obtain a glass frit;

[0126] d. After drying the obtained glass frit, put it into a ball mill for grinding to form a basic glass powder with an average particle size of 10 μm to 50 μm;

[0127] e. Mixing the base glass powder, colorant and lithium phosphate, wherein the lithium phosphate is added by dissolving in cold water and then drying, and then pressing and forming the mixture to obtain a green body;

[0128] f. The green body is heated to 700°C at a heating rate of 10°C / min and sintered in vacuum for 1 hour, after which the glass body is cooled in the furnace. The main component of the glass body obtained at this time is lithium disilicate, and the color of the semi-finished product is purple;

[0129] g. Finally, the semi-finished product is cut and placed in a porcelain furnace at a heating rate of 10°C / min. The temperature is raised to 880°C and kept at that temperature for 30 minutes. The finished product is then cooled in the furnace and the sintered product has a color close to that of real teeth.

[0130] After testing, the product has a strength of 394MPa, a crystallinity of 76.5%, and a phosphorus content of 0.19%.

[0131] Table 2 shows the performance test results of lithium disilicate glass ceramics prepared in Comparative Example 1 and Examples 1-7.

[0132] Table 2

[0133]

[0134] It can be seen from Comparative Example 1 and Examples 1 to 7 that the present invention uses lithium phosphate instead of phosphorus pentoxide as a nucleating agent, which not only avoids a large amount of mass waste, but also can produce lithium disilicate glass ceramics with lower strength, crystallinity and phosphorus content through this method.

[0135] It can be seen from Examples 3 and 6, and Examples 5 and 7 that the use of ammonia water to dissolve lithium phosphate in the present invention is better than cold water dissolution. Under the premise of the same addition amount, the sample obtained by dissolving with ammonia water has higher strength and crystallinity.

[0136] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a glass ceramic restoration, characterized in that: The following steps are involved: Providing a preparation raw material, which comprises, by mass percentage, 0.1% to 2% of lithium phosphate, 50% to 80% of silicon dioxide, 10% to 25% of lithium oxide, 2% to 8% of potassium oxide, 1% to 6% of aluminum oxide, 1% to 4% of zinc oxide, 0% to 6% of zirconium oxide, 0.5% to 3% of cerium oxide, 0.1% to 1% of vanadium pentoxide, 0.5% to 3% of erbium oxide and 0% to 0.5% of ferrosoferric oxide; The silicon dioxide, lithium oxide, potassium oxide, aluminum oxide, zinc oxide and zirconium oxide are uniformly mixed, and then melted, water quenched, dried and ground in sequence to obtain a basic glass powder; The basic glass powder, lithium phosphate, cerium oxide, vanadium pentoxide, erbium oxide and ferrosoferric oxide are uniformly mixed and then pressed to obtain a green body; The green body is sintered and then porcelain fired to obtain the glass ceramic restoration.

2. The method for preparing a glass ceramic restoration according to claim 1, characterized in that: The melting temperature is 1400°C to 1500°C.

3. The method for preparing a glass ceramic restoration according to claim 1 or 2, characterized in that: Before the basic glass powder, lithium phosphate and colorant are mixed evenly, the method further includes dissolving the lithium phosphate in a solvent and then drying it.

4. The method for preparing a glass ceramic restoration according to claim 1 or 2, characterized in that: The pressing molding is dry pressing molding, and the pressure of the dry pressing molding is 10MPa to 80MPa.

5. The method for preparing a glass ceramic restoration according to claim 1 or 2, characterized in that: The sintering is carried out under vacuum conditions, the sintering temperature is 700° C. to 800° C., and the heating rate is 5° C. / min to 10° C. / min.

6. The method for preparing a glass ceramic restoration according to claim 1 or 2, characterized in that: The temperature of the porcelain is 800° C. to 900° C., the heating rate is 5° C. / min to 10° C. / min, and the heat preservation time is 2 min to 30 min.

7. A glass ceramic restoration obtained by the method for preparing a glass ceramic restoration according to any one of claims 1 to 6.