A carboxylated graphene oxide / MOFs composite material and its preparation method and application

By composited graphene oxide with MOFs material under alkaline conditions, the carboxylated graphene oxide/MOFs composite material is solved, and the problems of poor stability and difficulty in recycling of adsorbents in the prior art are achieved, and efficient adsorption of heavy metal ions and Improved stability provides an effective method for removing heavy metals.

CN116099516BActive Publication Date: 2024-11-15GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310011752.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-05
Publication Date
2024-11-15
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

The existing heavy metal adsorbent materials have poor stability in actual applications, and powdered graphene oxide is difficult to recover, which limits its application effect.

Method used

Carboxylated graphene oxide/MOFs composite material is used to composite graphene oxide with MOFs material under alkaline conditions to form structural nodes of coordination bonds, improve the stability and hydrophilicity of the material, thereby improving adsorption performance.

Benefits of technology

The high-efficiency adsorption of heavy metal ions in water is achieved, the adsorption equilibrium is achieved within 20 minutes, the theoretical adsorption capacity is significantly improved, and the adsorption process conforms to the Langmuir isothermal model and the quasi-second rate equation, indicating that ion exchange and chemisorption are the main ones, providing An effective method for removing heavy metal ion is used.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116099516B_ABST
    Figure CN116099516B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of heavy metal adsorbent materials, and discloses a carboxyl graphene oxide / MOFs composite material and a preparation method and application thereof. The preparation method comprises the following steps: carboxylating graphene oxide under alkaline conditions to obtain carboxyl graphene oxide; activating the MOFs material, placing the carboxyl graphene oxide in an organic solvent, stirring and reacting the MOFs material at 95 to 105° C., and then freeze-drying the MOFs material to obtain the carboxyl graphene oxide / MOFs composite material. The carboxyl graphene oxide / MOFs composite material prepared by the method of the present invention can efficiently adsorb heavy metal ions of Pb(II), Cd(II), Cu(II), Ni(II), and Co(II) in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of heavy metal adsorbent materials, and in particular to a carboxyl graphene oxide / MOFs composite material and a preparation method and application thereof. Background Art

[0002] With the rapid development of modern economic society, mining, industrial metal smelting, electroplating and other industries have produced a large amount of heavy metals (referring to those with a density greater than 4.5g / cm 3 These heavy metals penetrate into the ecosystem in different forms, posing a serious threat to human health. For example, heavy metals such as copper, lead, zinc, cobalt, nickel, cadmium, and mercury cannot currently be eliminated through direct biodegradation.

[0003] In order to solve the above technical problems, researchers in this field have proposed some methods for removing heavy metal ions, such as chemical precipitation, separation, ion exchange, microbial treatment and adsorption. Among them, adsorption is considered to be one of the most effective methods for removing heavy metal ions due to its advantages such as simple operation, low energy consumption and no secondary pollution. Many adsorbents have been developed according to the adsorption principles of different materials, including chitosan, sulfide, activated carbon, montmorillonite, etc. Heavy metals are mainly removed through the interaction between adsorption materials and heavy metals. However, due to differences between adsorption materials, poor stability, and adaptation to the environment, there are still many problems in the actual application process.

[0004] In order to solve the above technical problems, researchers in this field have tried to use graphene-based materials to remove heavy metal ions, such as graphene oxide (GO). GO is an amphiphilic macromolecule that contains a large number of oxygen-containing functional groups on the basal plane or sheet edge, including hydroxyl, carboxyl and carbonyl groups, which can provide a large number of active sites. However, graphene oxide is mostly in powder form, and powdered GO is difficult to recycle in practical applications. This disadvantage limits its practical application.

[0005] To this end, the present invention provides a carboxyl graphene oxide / MOFs composite material and a preparation method and application thereof. Summary of the invention

[0006] In order to solve the deficiencies in the above-mentioned prior art, the present invention provides a carboxyl graphene oxide / MOFs composite material and its preparation method and application. The present invention uses a metal organic framework MOFs material as a carrier, and by compounding the MOFs material and the graphene-based material, the oxygen atoms in the graphene-based material and the metal ions in the MOFs will produce coordination bonds, which can act as structural nodes to participate in bonding interactions. The combination of these two materials can not only change the stability of the MOFs material, but also improve the hydrophilicity of the composite material to make it have better adsorption performance.

[0007] The carboxyl graphene oxide / MOFs composite material and its preparation method and application are achieved by the following technical solutions:

[0008] The first object of the present invention is to provide a method for preparing a carboxylated graphene oxide / MOFs composite material, comprising the following steps:

[0009] Step 1, carboxylating graphene oxide under alkaline conditions to obtain carboxylated graphene oxide;

[0010] Step 2, after activating the MOFs material, placing it in an organic solvent with the carboxylated graphene oxide, stirring and reacting it at 95-105° C., and then freeze-drying it to obtain the carboxylated graphene oxide / MOFs composite material.

[0011] Furthermore, the MOFs material is MOF-808.

[0012] Furthermore, the organic solvent is DMF.

[0013] Furthermore, the mass ratio of the MOFs material to the carboxyl graphene oxide is 1:4-6.

[0014] Furthermore, the usage ratio of the carboxylated graphene oxide to the organic solvent is 0.2-0.5 g:100 mL.

[0015] Furthermore, the activation temperature is 145-155° C., and the activation time is 12-36 hours.

[0016] Furthermore, the stirring reaction time is 6 to 10 hours, and the stirring rate is 250 to 300 r / min.

[0017] Furthermore, the freeze-drying temperature is -55 to -35°C, and the freeze-drying time is 12 to 36 hours.

[0018] The second object of the present invention is to provide a carboxylated graphene oxide / MOFs composite material prepared by the above preparation method.

[0019] The third object of the present invention is to provide an application of the above-mentioned carboxylated graphene oxide / MOFs composite material in the adsorption of heavy metal ions.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] In the present invention, under alkaline conditions, graphene oxide GO is subjected to an addition reaction to generate carboxylated graphene oxide GO-COOH, so that the surface of the graphene oxide exposes more active adsorption sites, and then GO-COOH is compounded with MOF-808 to obtain a GO-COOH / MOF-808 composite material.

[0022] The present invention preferably uses MOF-808, a MOFs material constructed with zirconium as the metal ion, as a carrier. MOF-808 has the advantages of large specific surface area, large pore size, and abundant metal center sites, which is conducive to forming coordination bonds with oxygen atoms in carboxyl graphene oxide, thereby generating a composite material cross-linked by chemical bonds, which can not only improve the stability of the MOFs material, but also improve the hydrophilicity of the composite material to make it have better adsorption performance.

[0023] The GO-COOH / MOF-808 composite material obtained by the present invention can efficiently adsorb Pb in water. 2+ , Cd 2+ , Cu 2+ , Ni 2 + ,Co 2+ Heavy metal ions can reach adsorption equilibrium within 20 minutes, and the theoretical adsorption capacities are 173.31 mg / g, 149.25 mg / g, 86.21 mg / g, 95.79 mg / g, and 88.73 mg / g, respectively. The adsorption effect is significant. Moreover, the adsorption process is consistent with the Langmuir isotherm model and the pseudo-second-order rate equation, indicating that the adsorption process is mainly based on ion exchange and chemical adsorption. The possible mechanisms of heavy metal ion adsorption analyzed by FTIR and XPS include ion exchange, electrostatic adsorption, chemical adsorption, π-π interaction, and coordination complexation. The results show that GO-COOH / MOF-808 prepared by the present invention is an effective adsorbent that is expected to remove heavy metal ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The results of the adsorption capacity test of different adsorbent materials for heavy metal ions;

[0025] Figure 2 The test results of the adsorption capacity of the composite material of Example 1 for heavy metal ions at different pH values;

[0026] Figure 3 The adsorption capacity test results of the composite material of Example 1 for heavy metal ions at different adsorption times;

[0027] Figure 4 The adsorption capacity test results of the composite material of Example 1 for heavy metal ions of different concentrations;

[0028] Figure 5 For Figure 3 The pseudo first-order rate equation obtained by fitting the test results;

[0029] Figure 6 For Figure 3 The pseudo-second-order rate equation obtained by fitting the test results;

[0030] Figure 7 For Figure 4 The test results were fitted to the Langmuir equation;

[0031] Figure 8 For Figure 4 The test results were fitted to the obtained Freundlich equation;

[0032] Fig. 9 The adsorption capacity test results of the composite material of Example 1 after different cycle times;

[0033] Fig.10 The EDS test results of the composite material of Example 1 after adsorbing heavy metal ions;

[0034] Fig.11 Schematic diagram of the adsorption mechanism of the composite material of the present invention. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0036] The present invention provides a carboxyl graphene oxide / MOFs composite material, and the preparation method thereof is as follows:

[0037] Step 1, carboxylating graphene oxide to obtain carboxylated graphene oxide;

[0038] It should be noted that the present invention does not limit the specific method of carboxylating graphene oxide, as long as carboxylated graphene oxide can be obtained. Preferably, the following steps (S1-S4) are used to carboxylate graphene oxide:

[0039] S1, uniformly dispersing graphene oxide in an aqueous solvent to obtain a graphene oxide solution;

[0040] The ratio of graphene oxide to water solvent is 0.05-0.15 g:100 mL. The present invention does not limit the specific method of dispersing graphene oxide in water solvent, as long as the graphene oxide can be evenly dispersed in the water solvent. In the present invention, it is preferred to disperse by ultrasound, and the ultrasound frequency is 600 W, and the power is 40 KHz under ultrasound conditions for 1-3 hours.

[0041] S2, adding a base and a carboxyl source to the graphene oxide solution, and performing ultrasonic treatment to obtain a mixture A;

[0042] Wherein, the dosage ratio of the base to the graphene oxide content in the graphene oxide solution is 12.5mmol:0.05-0.15g; the dosage ratio of the carboxyl group in the carboxyl source to the graphene oxide content in the graphene oxide solution is 5.3mmol:0.05-0.15g. In addition, the present invention takes into account that under strong alkaline conditions, the hydroxyl (-OH) and epoxy (COC) distributed on the GO basal surface and the carboxyl (-COOH) contained on the edge are easily subjected to nucleophilic substitution reaction with chloroacetic acid, and finally the epoxy and hydroxyl groups on the GO surface are converted into carboxymethyloxy groups. Sodium hydroxide is used as an alkali agent and chloroacetic acid is used as a carboxyl source, which are sequentially added to the graphene oxide solution, and then the graphene oxide is treated under the action of ultrasound.

[0043] S3, adding an acid to the mixture A to adjust its pH to neutral, to obtain a mixture B;

[0044] The present invention does not limit the type and concentration of the acid used, as long as the pH of the solution system is adjusted to neutral (pH=7). For example, 1 mol / L hydrochloric acid can be used for adjustment.

[0045] S4, repeatedly washing the mixture B with water and centrifuging to wash away excess salt and sodium hydroxide, until the washing solution is neutral, to obtain solid A, and after drying solid A, to obtain solid B, wherein solid B is the carboxyl graphene oxide;

[0046] Among them, the present invention preferably uses freeze drying to dry solid A, so that solid A is dried in a frozen state, so that the volume of the dried product remains almost unchanged, the original structure is still maintained, and no concentration occurs. The dried product is loose and porous, and is sponge-like, which is conducive to its later compounding with MOFs materials. The freeze drying temperature of the present invention is -55 to -35°C, and the freeze drying time is 12 to 36 hours.

[0047] Step 2, after activating the MOFs material, placing it in an organic solvent with the carboxylated graphene oxide, stirring and reacting it at 95-105° C., and then freeze-drying it to obtain the carboxylated graphene oxide / MOFs composite material;

[0048] It should be noted that the present invention preferably activates the MOFs material at 145-155° C. for 12-36 hours, so that the MOFs material is in an active state through high temperature treatment, which is convenient for compounding with carboxyl graphene oxide.

[0049] In order to make the MOFs material and the carboxylated graphene oxide fully contact and react under solvent conditions, the present invention preferably uses DMF as the reaction solvent, and the mass ratio of the MOFs material to the carboxylated graphene oxide is 1:4-6, and the amount ratio of the carboxylated graphene oxide to the organic solvent is 0.2-0.5g:100mL. The activated MOFs material and the carboxylated graphene oxide are placed in the DMF solvent for stirring reaction.

[0050] In order to quickly and evenly disperse the MOFs material and the carboxylated graphene oxide, the present invention preferably stirs at a stirring rate of 250 to 300 r / min for 6 to 10 hours, so that the activated MOFs material and the carboxylated graphene oxide are fully contacted and reacted in DMF.

[0051] In order to improve the adsorption performance of the obtained carboxyl graphene oxide / MOFs composite material, the present invention further freeze-dries the product obtained after the stirring reaction, and the freeze-drying temperature is -55 to -35°C, and the freeze-drying time is 12 to 36 hours, so that the solid A is dried in a frozen state, so that the volume of the dried product is almost unchanged, the original structure is still maintained, and no concentration phenomenon occurs. In addition, the dried product is loose and porous, and is sponge-like, which is conducive to increasing its specific surface area and porosity, and improving its adsorption performance when used as an adsorption material.

[0052] Example 1

[0053] This embodiment provides a carboxyl graphene oxide / MOFs composite material, and the preparation method thereof is as follows:

[0054] 1) Preparation of carboxylated graphene oxide

[0055] 0.1g GO was added to 100ml distilled water and ultrasonically irradiated for 2h to obtain graphene oxide solution. Then 0.5g NaOH and 0.5g ClCH2COOH were added and ultrasonicated for 2h to make it uniformly dispersed. Finally, 1M HCl was added until the pH of the solution reached 7. The stirring process was continued until there was no particle feeling, and the solution was repeatedly washed and centrifuged with deionized water. The powder was freeze-dried in a -45℃ freeze dryer for 24h to obtain carboxyl graphene oxide, which was recorded as GO-COOH.

[0056] 2) Preparation of MOFs materials

[0057] In this embodiment, MOF-808 is used as the MOFs material, and it is prepared by the following steps:

[0058] ZrOCl2·8H2O (322 mg, 1.0 mmol) and H3BTC (210 mg, 1.0 mmol) were completely dissolved in a solvent mixture of DMF / formic acid (40 mL / 40 mL), then placed in a 100 ml polytetrafluoroethylene reactor and heated at 130 ° C for 48 h. The reaction mixture was soaked in DMF and methanol, washed repeatedly with EtOH and distilled water, and then freeze-dried in a -45 ° C freeze dryer for 24 h to obtain MOF-808 powder.

[0059] 3) Composite carboxyl graphene oxide and MOFs materials

[0060] First, activate MOF-808 at 145-155°C for 12-36h.

[0061] Then GO-COOH and MOF-808 were transferred to a round-bottom flask containing N,N-dimethylformamide (DMF) in a mass ratio of 5:1, and the mixture was stirred at 100°C at a stirring rate of 280r / min for 8h. The solution was repeatedly washed with DMF / methanol and distilled water. Thereafter, the product was freeze-dried in a -45°C freeze dryer for 24h. Functionalized grafted GO-COOH / MOF-808 was obtained.

[0062] Example 2

[0063] This embodiment provides a carboxyl graphite oxide / MOFs composite material, and its preparation method is different from that of embodiment 1 only in that:

[0064] The mass ratio of GO-COOH and MOF-808 is 1:13.

[0065] Example 3

[0066] This embodiment provides a carboxyl graphite oxide / MOFs composite material, and its preparation method is different from that of embodiment 1 only in that:

[0067] The mass ratio of GO-COOH and MOF-808 is 1:5.

[0068] Example 4

[0069] This embodiment provides a carboxyl graphite oxide / MOFs composite material, and its preparation method is different from that of embodiment 1 only in that:

[0070] The mass ratio of GO-COOH and MOF-808 is 1:1.

[0071] Example 5

[0072] This embodiment provides a carboxyl graphite oxide / MOFs composite material, and its preparation method is different from that of embodiment 1 only in that:

[0073] The mass ratio of GO-COOH and MOF-808 is 13:1.

[0074] Example 6

[0075] This embodiment provides a carboxyl graphite oxide / MOFs composite material, and its preparation method is different from that of embodiment 1 only in that:

[0076] The mass ratio of GO-COOH and MOF-808 is 4:1.

[0077] Example 7

[0078] This embodiment provides a carboxyl graphite oxide / MOFs composite material, and its preparation method is different from that of embodiment 1 only in that:

[0079] The mass ratio of GO-COOH and MOF-808 is 6:1.

[0080] Example 8

[0081] This embodiment provides a carboxyl graphite oxide / MOFs composite material, and its preparation method is different from that of embodiment 1 only in that:

[0082] Step 1) When preparing carboxylated graphene oxide, the amount of graphene oxide GO is 0.05 g, the amount of NaOH is 0.25 g, and the amount of ClCH2COOH is 0.25 g; and the ultrasonic treatment time is 1 h;

[0083] The freeze-drying temperature was -55°C and the freeze-drying time was 12 h.

[0084] Step 3) When preparing the composite carboxyl graphene oxide and MOFs material, the activation temperature of MOF-808 is 145° C. and the activation time is 12 h;

[0085] The stirring reaction temperature was 95°C, the stirring rate was 250 r / min, and the stirring time was 6 h;

[0086] The freeze-drying temperature was -55°C and the freeze-drying time was 12 h.

[0087] Example 9

[0088] This embodiment provides a carboxyl graphite oxide / MOFs composite material, and its preparation method is different from that of embodiment 1 only in that:

[0089] Step 1) When preparing carboxylated graphene oxide, the amount of graphene oxide GO is 0.15 g, the amount of NaOH is 0.5 g, and the amount of ClCH2COOH is 0.5 g; and the ultrasonic treatment time is 3 h;

[0090] The freeze-drying temperature was -35°C and the freeze-drying time was 36 h.

[0091] Step 3) When preparing the composite carboxyl graphene oxide and MOFs material, the activation temperature of MOF-808 is 155° C. and the activation time is 36 h;

[0092] The stirring reaction temperature was 105°C, the stirring rate was 300 r / min, and the stirring time was 10 h;

[0093] The freeze-drying temperature was -35°C and the freeze-drying time was 36 h.

[0094] Experimental Section

[0095] (I) Effect of different ratios of GO-COOH and MOF-808 on the adsorption effect of the composite material of the present invention

[0096] The present invention uses the GO-COOH / MOF-808 composite materials prepared in Examples 1 to 5 as adsorbents, and uses graphene oxide, carboxyl graphene oxide and MOF-808 as comparative adsorbents to test the adsorption capacity of heavy metal ions Pb(II), Cd(II), Cu(II), Ni(II) and Co(II). The test results are as follows: Figure 1 shown.

[0097] And the test conditions are as follows:

[0098] Eight groups of 20 mL Pb(II), Cd(II), Cu(II), Ni(II), and Co(II) heavy metal ion solutions with a heavy metal ion concentration of 100 mg / g and a pH of 6.5 were taken as wastewater to be treated containing heavy metal ions, and 10 mg of each of the above adsorbents was added respectively. After stirring the reaction at a stirring rate of 200 r / min for 2 hours, the adsorption capacity was tested.

[0099] Depend on Figure 1is the adsorption capacity of GO-COOH / MOF-808 at different ratios. It can be seen that the adsorption capacity (mg / g) of single carboxylated graphene oxide for Pb(II), Cd(II), Cu(II), Ni(II) and Co(II) heavy metal ions are 104, 99.8, 62.7, 65.97 and 72.03 respectively; the adsorption capacity (mg / g) of single MOF-808 for Pb(II), Cd(II), Cu(II), Ni(II) and Co(II) heavy metal ions are 73.41, 23.34, 37.98, 18.3 and 20.55 respectively; the adsorption effect of the composite material of Example 1 is the best, and its adsorption capacity (mg / g) for Pb(II), Cd(II), Cu(II), Ni(II) and Co(II) heavy metal ions are 156, 135, 91.49, 90.99 and 82.02 respectively.

[0100] The composite material of the present invention has significantly improved adsorption effect compared with single carboxylated graphene oxide (GO-COOH) and single MOF-808, which may be because in the composite material of the present invention, the carboxyl group and epoxy group in the carboxylated graphene oxide can be combined with the Zr group in MOF-808 to form a composite material with chemical bonding, which can improve the activity of the adsorption site, so that the obtained composite material has ion exchange, coordination complexation, π-π bond, electrostatic adsorption, chemical adsorption and other forms of adsorption, thereby achieving improvement in the adsorption performance of the composite material.

[0101] Furthermore, by comparing the changes in adsorption capacity of Example 1-Example 5, it can be seen that the ratio of carboxylated graphene oxide to MOF-808 has a significant effect on its adsorption capacity, and when the carboxylated graphene oxide is too little, it cannot be fully combined with the surface of MOF-808, which easily leads to large-area accumulation of MOF materials, which is not conducive to adsorption, and too much MOF-808 will also occupy the adsorption sites of carboxylated graphene oxide, thereby causing the adsorption performance of the composite material to be greatly reduced, even lower than the adsorption performance of a single material. When there are too many carboxylated graphene oxides, they are too loosely combined with MOF-808, and it is impossible to fully make carboxylated graphene oxide and MOF-808 synergistic, resulting in poor adsorption performance. And the present invention takes into account that the adsorption effect is different and is related to the number of adsorption groups and the activity of adsorption sites. In order to give full play to the adsorption effects of various forms such as composite material ion exchange, coordination complexation, π-π bond, electrostatic adsorption, and chemical adsorption, the mass ratio of the preferred MOFs material to carboxylated graphene oxide in the present invention is 1:4-6.

[0102] (II) Effect of different pH on the adsorption effect of the composite material of the present invention

[0103] The present invention takes the composite material of Example 1 as an example to explore the influence of pH on the adsorption effect of the composite material of the present invention, and the test results are as follows Figure 2 It should be noted that in order to avoid the formation of various precipitations due to excessively high pH, ​​the initial pH was selected to be 1-6 when exploring the relationship between pH and adsorption capacity, and the pH value was adjusted using 0.5M HCl and 0.5M NaOH solutions throughout the process. And the test conditions are:

[0104] Six groups of 20 mL of Pb(II), Cd(II), Cu(II), Ni(II), and Co(II) heavy metal ion solutions with a heavy metal ion concentration of 100 mg / g and different pH values ​​(pH 1, 2, 3, 4, 5, and 6) were taken as wastewater to be treated containing heavy metal ions, and 10 mg of the composite material of Example 1 was added as an adsorbent. After stirring the reaction at a stirring rate of 200 r / min for 2 hours, the adsorption capacity was tested.

[0105] Figure 2 is the adsorption capacity of the composite material prepared in Example 1 of the present invention at different pH values, and Figure 2 It can be seen that when the pH is between 1 and 3, the adsorption capacity of the composite material prepared in Example 1 is very low. This is because the GO-COOH / MOF-808 material structure contains benzene ternary ligands, and the unsaturated functional groups will cause the water environment to be acidic, and many heavy metal ions will react with H + Competition for adsorption sites on the composite material resulted in a lower adsorption capacity. The adsorption amount also increased dramatically between pH 3 and 5, which was attributed to the generation of more COO- groups. + As the concentration continues to decrease, competitive adsorption will be reduced. In addition, the increase in the pH value of the solution will lead to the deprotonation of the benzene ternary ligand, and the deprotonated oxygen-containing functional groups can enhance the coordination and complexation with metal cations, and the adsorption capacity will increase. The pH value tends to be balanced between 5 and 6. This is because the active sites occupied by heavy metal ions in the composite material have reached the saturation value, and its adsorption capacity will not change significantly. Therefore, the experimental condition of pH 5.5 was used in the later experiments.

[0106] (III) Effect of different adsorption times on the adsorption effect of the composite material of the present invention

[0107] The present invention takes the composite material of Example 1 as an example to explore the influence of different adsorption times on its adsorption effect, and the test results are as follows Figure 3 shown.

[0108] Figure 3The adsorption capacity of the composite material for Pb(II), Cd(II), Cu(II), Ni(II), and Co(II) at different times shows that, with the passage of time, the capacity of the composite material for adsorbing heavy metal ions increases continuously, and the adsorption equilibrium is reached in about 20 minutes. Therefore, the present invention preferably uses the composite material of the present invention to adsorb heavy metal ions, and the adsorption treatment can be stopped after 20 minutes of action, so the adsorption treatment takes a short time and has a high adsorption efficiency.

[0109] (IV) Effect of different heavy metal ion concentrations on the adsorption effect of the composite material of the present invention

[0110] The present invention takes the composite material of Example 1 as an example, and takes six groups of 20mL of Pb(II), Cd(II), Cu(II), Ni(II), Co(II) heavy metal ion solutions with different heavy metal ion concentrations (50mg / g, 100mg / g, 150mg / g, 200mg / g, 250mg / g, 300mg / g, 350mg / g and 400mg / g) and pH 6.5 as the wastewater to be treated containing heavy metal ions, and adds 10mg of the composite material of Example 1 as an adsorbent, and stirs the reaction at a stirring rate of 200r / min for 2h, and then tests its adsorption capacity to explore the influence of different heavy metal ion concentrations on its adsorption effect, and the test results are as follows: Figure 4 shown.

[0111] Figure 4 The adsorption capacity of the composite material of Example 1 of the present invention for Pb(II), Cd(II), Cu(II), Ni(II) and Co(II) under different heavy metal ion concentrations. It can be seen that the adsorption capacity obtained by placing the same composite material under different heavy metal ion concentration conditions is different, and the adsorption capacity is the largest under the condition of ion concentration of 100 mg / g.

[0112] The present invention is based on Figure 3 The test results of the relationship between time and adsorption capacity were fitted to obtain the pseudo first-order rate equation and pseudo second-order rate equation, as shown in Figure 5 and Figure 6 As shown, and by comparison Figure 5 and Figure 6 It can be seen that the composite material of Example 1 of the present invention adsorbs heavy metal ions in the form of ion exchange and chemical adsorption.

[0113] The present invention is based on Figure 4 The test results of the relationship between the concentration and the adsorption capacity were fitted to obtain the Langmuir equation and the Freundlich equation, respectively. Figure 7 and Figure 8 As shown, and by comparison Figure 7 and Figure 8 It can be seen that the adsorption of the composite material of Example 1 of the present invention includes monolayer adsorption on specific functional groups.

[0114] (V) Relationship between cycle number and adsorption capacity

[0115] The present invention takes the composite material of Example 1 as an example to explore the relationship between the number of cycles and the adsorption capacity, and the test results are as follows Fig. 9 shown.

[0116] Depend on Fig. 9 It can be seen that the composite material of the present invention still has a relatively high adsorption capacity after being recycled three times, which indicates that the composite material of the present invention has good adsorption performance and can be recycled.

[0117] (VI) EDS test

[0118] The present invention takes the composite material of Example 1 as an example, and conducts EDS test after adsorbing Pb(II), Cd(II), Cu(II), Ni(II), and Co(II). The test results are as follows: Fig.10 As shown, Fig.10 In the figure, a is the EDS image of the composite material of Example 1, b is the distribution of adsorbed Pb(II), c is the distribution of adsorbed Cd(II), d is the distribution of adsorbed Cu(II), e is the distribution of adsorbed Ni(II), and f is the distribution of adsorbed Co(II).

[0119] Depend on Fig.10 It can be seen that heavy metal ions such as Pb(II), Cd(II), Cu(II), Ni(II), Co(II) are evenly distributed on the surface of the composite material, indicating that the composite material prepared by the present invention has very uniform components and can evenly adsorb heavy metal ions in multiple directions.

[0120] Based on the above, the composite material of the present invention may be obtained by Fig.11 The ion exchange, coordination complexation, π-π, electrostatic adsorption, chemical adsorption and other adsorption effects shown work together to achieve the adsorption effect, and realize the adsorption of Pb(II), Cd(II), Cu(II), Ni(II), and Co(II).

[0121] The above embodiments are only for illustrating the technical idea of ​​the present invention, and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the present invention; any technology not involved in the present invention can be realized by existing technologies.

[0122] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. Application of a carboxyl graphene oxide / MOFs composite material in adsorbing lead ions, characterized in that: The preparation method of the carboxyl graphene oxide / MOFs composite material comprises the following steps: Step 1, carboxylating graphene oxide to obtain carboxylated graphene oxide; Step 2, after activating the MOFs material, placing it in an organic solvent with the carboxyl graphene oxide, then stirring and reacting at 95-105° C., and then freeze-drying to obtain the carboxyl graphene oxide / MOFs composite material; The MOFs material is MOF-808; The mass ratio of the MOFs material to the carboxyl graphene oxide is 1:4-6; The activation temperature is 145-155° C., and the activation time is 12-36 hours.

2. The use according to claim 1, characterized in that The organic solvent is DMF.

3. The use according to claim 1, characterized in that The usage ratio of the carboxylated graphene oxide to the organic solvent is 0.2-0.5 g:100 mL.

4. The use according to claim 1, characterized in that The stirring reaction time is 6-10 hours, and the stirring rate is 250-300 r / min.

5. The use according to claim 1, characterized in that The freeze drying temperature is -55 to -35°C, and the freeze drying time is 12 to 36 hours.