A non-precious metal copper modified carbon-based composite material and its preparation method and application

By modifying the three-dimensional structure and photoelectron transfer mechanism of carbon-based composite materials with non-precious metal copper, the problem of disinfection byproducts and loss of nano-copper during water sterilization was solved, achieving rapid and efficient water disinfection.

CN116099550BActive Publication Date: 2024-11-12ZHEJIANG UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211389815.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-08
Publication Date
2024-11-12
Estimated Expiration
2042-11-08

AI Technical Summary

Technical Problem

Existing water sterilization methods suffer from problems such as the generation of disinfection byproducts, high energy consumption, or incomplete sterilization, and the loss of nano-copper materials in water is serious.

Method used

A non-precious metal copper-modified carbon-based composite material is used. A three-dimensional structure is formed by the self-assembly of sulfur-zinc-indium sheets and carbon-based materials. Nanoscale copper particles are anchored by room temperature in-situ photodeposition. Combined with visible light-excited photoelectron transfer and copper ion regeneration, the loss of nano-copper is reduced and the sterilization performance is enhanced.

Benefits of technology

It achieves rapid and effective inactivation of harmful microorganisms in water under visible light irradiation, avoids the generation of disinfection byproducts, improves the stability and dispersibility of nano-copper, and provides an efficient alternative technology for water disinfection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116099550B_ABST
    Figure CN116099550B_ABST
Patent Text Reader

Abstract

The invention discloses a non-precious copper modified carbon-based composite material and its preparation method and application. The preparation method comprises the following steps: dissolving zinc salt, indium salt and sulfur source in water respectively, adjusting the pH of the mixed solution to 0.5-5, introducing carbon-based material, hydrothermal reaction, washing after centrifugal separation of precipitate to obtain dark yellow solid, placing in a vacuum oven and drying overnight, and obtaining a carbon-based sulfur-indium-zinc composite material; the prepared copper ion solution mixed composite material is subjected to photodeposition reaction to obtain a nano-copper modified sulfur-indium-zinc / carbon-based composite material; centrifugal washing and drying to obtain a non-precious copper modified carbon-based composite material. The sulfur-zinc-indium in the composite material of the present invention absorbs the copper ions released by the photoelectrons excited by visible light and transmitted by the carbon-based material, reduces the loss of copper, improves the stability and dispersibility of nano-copper particles, and strengthens the bactericidal ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of preparation of bactericidal composite materials, and in particular relates to a non-precious metal copper-modified carbon-based composite material and a preparation method and application thereof. Background Art

[0002] Polluted water contains a large number of harmful bacteria, which will have a serious impact on the ecological environment if they enter the environment. Traditional water sterilization methods include chlorination, ozone, and ultraviolet disinfection. Chlorination disinfection has the advantages of stability and high efficiency, but studies have shown that the disinfection byproducts it produces will increase the incidence of cancer and even damage the central nervous system; ultraviolet disinfection is efficient and clean, but it has high energy consumption, there are bacteria that cannot be completely killed, photoregeneration occurs, and enhanced genes are formed.

[0003] Researchers have found that some nanomaterials with specific structures or precious metals and their compounds have the ability to destroy or affect cell structure, metabolism, etc. to achieve sterilization. Common nano sterilization materials are mainly the following: metal and metal oxide nanomaterials, sulfur-based nanomaterials, carbon-based nanomaterials, and nitrogen-based nanomaterials. In the sterilization process of nanomaterials, there are sterilization mechanisms such as metal ion release, physical damage, and oxidative stress. Because of its high efficiency, strong bactericidal ability, good durability, and less secondary pollution, it is considered to be one of the best candidates for fighting pathogens. Ag has a good sterilization effect, is relatively stable and long-lasting, and is the most widely used nano sterilization material, but the high cost of precious metals as it is lost is a hard flaw. In comparison, nano copper (CuNPs), as a transition metal element, is cheap and easy to obtain, and is a trace element necessary for normal human metabolism. Kumar et al. applied a shellac / copper nanoparticle (CuNPs) nanocoating composite to a non-woven surgical mask, using the sterilization ability of nano-copper to make the mask reusable and self-sterilizable (Nano Letters, 2021, 337-343). However, like other metal materials, Cu 2+ It can also be lost in bodies of water.

[0004] Compared with single metal materials, multi-component composite functional materials based on nanometals can show better comprehensive efficacy through the synergistic effect between components, which can improve the stability and dispersibility of nanometal particles and reduce their loss. Song et al. modified reduced graphene oxide (Ag / rGO) with nanosilver particles in situ, and the material showed significant bactericidal ability (99.9%) against Gram-negative Escherichia coli (Applied Surface Science, 2019, 682). The three-phase composite material rGO-AgNP / Bi2Fe4O9 prepared by Hu et al. showed super-efficient bactericidal effect on Gram-negative Escherichia coli, Pseudomonas aeruginosa and Gram-positive Staphylococcus aureus (Applied Catalysis B, 2018, 548). In addition, composite materials are conducive to improving the activity of each component material and are one of the important development directions of functional materials. Summary of the invention

[0005] In order to overcome the shortcomings and deficiencies in the prior art, the object of the present invention is to provide a non-precious metal copper modified carbon-based composite material and a preparation method and application thereof.

[0006] In order to achieve the above objectives, the following technical solutions are proposed:

[0007] A method for preparing a non-precious metal copper-modified carbon-based composite material comprises the following steps:

[0008] 1) Dissolve the zinc salt, indium salt and sulfur source in water respectively, mix them in sequence, stir them magnetically to obtain a mixed solution, adjust the pH of the mixed solution with an acidic solution, introduce the carbon-based material, continue stirring, and after the stirring is completed, transfer the mixed solution to a hydrothermal reactor, and move it to an oven for reaction;

[0009] 2) After the reaction is completed, the reaction is cooled to room temperature, the precipitate is centrifuged and then washed with ultrapure water and anhydrous ethanol to obtain a dark yellow solid, which is then placed in a vacuum oven and dried overnight to obtain a sulfur-indium-zinc / carbon-based composite material;

[0010] 3) dissolving copper salt in ultrapure water, ultrasonically preparing a copper ion solution for later use, ultrasonically dispersing the sulfur indium zinc / carbon-based composite material prepared in step 2) in water, mixing it with the prepared copper ion solution, and transferring it into a photoreactor after ultrasonic treatment, bubbling nitrogen to remove dissolved oxygen, and slowly injecting a reducing solution under magnetic stirring and light irradiation, and performing a photodeposition reaction for 5-180 min to obtain a nano-copper-modified sulfur indium zinc / carbon-based composite material;

[0011] 4) The nano-copper modified sulfur indium zinc / carbon-based composite material prepared in step 3) is centrifuged, washed with ultrapure water and anhydrous ethanol to remove residual salt, and dried in a vacuum oven overnight to obtain a non-precious metal copper modified carbon-based composite material.

[0012] Furthermore, the carbon-based material in step 1) is a mixture of one or more of carbon nanotubes, graphene and biochar, and the amount of the carbon-based material added is 0.1-10% of the mass of sulfur indium zinc.

[0013] Further, the zinc salt in step 1) is zinc chloride, zinc nitrate, zinc sulfate, zinc phosphate, zinc acetate, zinc citrate, zinc isooctanoate or zinc glycinate, the indium salt is indium chloride, indium nitrate, indium sulfate, indium phosphate, indium acetate or indium citrate, the sulfur source is thioacetamide, ammonium sulfide, thiourea or sodium thiosulfate, the acidic solution is hydrochloric acid, sulfuric acid, phosphoric acid, acetic acid, citric acid, sulfonic acid or salicylic acid, and the concentration of the acidic solution is 0.5-8 mol / L.

[0014] Furthermore, the molar ratio of the zinc salt, the indium salt and the sulfur source in step 1) is 1-1.5:2-3:4-6.

[0015] Furthermore, the copper salt described in step 3) is copper chloride, copper nitrate, copper phosphate, copper acetate or sodium copper ethylenediaminetetraacetate, and the amount of copper salt added is 0.5-20% of the mass of the zinc indium sulfide / carbon-based composite material.

[0016] Furthermore, the reducing solution in step 3) is hydrazine, sodium borohydride, potassium borohydride, ethanol, ammonia water or sodium sulfite, the concentration of the reducing solution is 0.01-0.6 mol / L, the molar ratio with the copper salt is 3-15:1, and the injection speed of the reducing solution is 2-3 drops / second.

[0017] Furthermore, the magnetic stirring time in step 1) is 2-120 min, the pH of the solution is adjusted to 0.5-5, the carbon-based material is introduced, stirring is continued for 1-24 hours, the reaction temperature in the oven is 100-220° C., and the reaction time is 6-48 hours.

[0018] A non-noble metal copper modified carbon-based composite material prepared by the above preparation method.

[0019] The application of the above-mentioned non-precious metal copper modified carbon-based composite material is to place the non-precious metal copper modified carbon-based composite material in a water body containing harmful bacteria. Under visible light irradiation, a constant temperature water bath is used to maintain the water body at room temperature, and PBS buffer is used to maintain the water body pH at 7.4. The pathogens in the water body are disinfected by multiphase catalysis. After the disinfection reaction is completed, the non-precious metal copper-based composite material is separated and recovered.

[0020] The beneficial effects of the present invention are:

[0021] 1) The present invention uses a self-assembled three-dimensional structure of sulfur-zinc-indium flake fusion carbon-based materials as a carrier and adopts a room-temperature in-situ photodeposition method to anchor nano-scale copper particles, which effectively avoids the agglomeration of nano-copper and improves the stability and dispersibility of nano-copper particles.

[0022] 2) During the disinfection process, the non-precious metal copper-based composite functional material of the present invention can in situ regenerate the released copper ions through the transfer of photoelectrons excited by visible light absorbed by sulfur, zinc and indium through carbon-based materials, thereby effectively reducing the loss of CuNPs; on the other hand, it inhibits the recombination of photogenerated electron-hole pairs of sulfur, zinc and indium, and comprehensively enhances the disinfection and sterilization performance of the material.

[0023] 3) The composite functional material prepared by the present invention is used for disinfecting harmful microorganisms. It can quickly and effectively inactivate harmful microorganisms in water under visible light irradiation, truly avoiding the unavoidable practical problem of producing disinfection by-products in traditional water disinfection, and opening up new ideas for the development of alternative technologies for drinking water disinfection. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 XRD patterns of Cu-ZIS / CNTs composite material, ZnIn2S4 and Cu-ZnIn2S4 prepared in Example 1;

[0025] Figure 2 N2 physical adsorption-desorption curves of Cu-ZIS / CNTs composite material and ZnIn2S4 prepared in Example 1;

[0026] Figure 3 TEM image of the Cu-ZIS / CNTs composite material prepared in Example 1;

[0027] Figure 4 This is a comparison chart of the sterilization effects of different materials on the target pathogen Pseudomonas aeruginosa;

[0028] Figure 5 This is a comparison chart of the effects of the Cu-ZIS / CNTs composite material of the present invention on catalytic disinfection and sterilization of Pseudomonas aeruginosa, Escherichia coli, and Staphylococcus aureus;

[0029] Figure 6 This is the cyclic disinfection efficiency diagram of the Cu-ZIS / CNTs composite material prepared in Example 1. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0031] Example 1

[0032] Preparation of Cu-ZIS / CNTs composites:

[0033] 1) Dissolve 0.068g ZnCl2, 0.239g InCl2·4H2O and 0.15g CH3CSNH2 in water respectively, mix and stir in sequence, and stir magnetically for 30min to form 40mL mixed metal salt solution A; adjust the pH of the mixed solution A to 1.0 with 5M HCl solution; then weigh 2mg carbon nanotubes and add them to solution A, and continue stirring for 12h to obtain a mixed solution B; then transfer the mixed solution B to a hydrothermal reactor with a polytetrafluoroethylene liner; seal the hydrothermal reactor and put it in an oven, heat it to 160℃ and keep it for 16h; after the reaction is completed, cool it to room temperature, centrifuge the precipitate, wash it several times with ultrapure water and anhydrous ethanol to obtain a dark yellow solid, and place it in a vacuum oven at 60℃ and vacuum dry it for 12h to obtain a three-dimensional nanostructured ZnIn2S4 / CNTs composite functional material;

[0034] 2) Dissolve 4.2 mg CuCl2 in 5 mL ultrapure water, and ultrasonically prepare a copper ion solution for later use; dissolve 14.3 mg NaBH4 in 5 mL ultrapure water, and ultrasonically prepare a sodium borohydride aqueous solution for later use; ultrasonically disperse 100 mg of the ZnIn2S4 / CNTs composite material obtained in step 1) in 40 mL of water, and ultrasonically disperse it evenly, mix it with the prepared copper ion solution, and move it into a quartz photoreactor after ultrasonication, and drive away the dissolved oxygen with nitrogen bubbling. Under magnetic stirring and illumination, slowly inject the sodium borohydride aqueous solution at a rate of 2 drops / second, and terminate the photodeposition reaction after 60 minutes, during which the room temperature is maintained in a constant temperature water bath; after the reaction, the sample is centrifuged, washed with ultrapure water and anhydrous ethanol to remove residual salt, and dried in a vacuum oven at 60°C for 12 hours to obtain the non-precious metal copper-based composite material, which is marked as Cu-ZIS / CNTs composite material.

[0035] Preparation of ZnIn2S4 material:

[0036] 0.068g ZnCl2, 0.239g InCl2·4H2O and 0.15g CH3CSNH2 were dissolved in water respectively, mixed and stirred in turn, and magnetically stirred for 30min to form 40mL mixed metal salt solution A; the mixed solution A was transferred to a hydrothermal reactor with a polytetrafluoroethylene liner; the hydrothermal reactor was sealed and placed in an oven, heated to 160℃ and maintained for 16h; after the reaction was completed, it was cooled to room temperature, the precipitate was centrifuged and washed several times with ultrapure water and anhydrous ethanol to obtain a dark yellow solid, which was placed in a vacuum oven at 60℃ and vacuum dried for 12h, namely ZnIn2S4 material.

[0037] Preparation of Cu-ZnIn2S4 material:

[0038] Dissolve 4.2 mg CuCl2 in 5 mL ultrapure water, and prepare a copper ion solution by ultrasonication for later use; dissolve 14.3 mg NaBH4 in 5 mL ultrapure water, and prepare a sodium borohydride aqueous solution by ultrasonication for later use; ultrasonically disperse 100 mg ZnIn2S4 material in 40 mL water, disperse it evenly by ultrasonication, mix it with the prepared copper ion solution, and transfer it into a quartz photoreactor after ultrasonication, and drive away the dissolved oxygen by nitrogen bubbling. Under magnetic stirring and illumination, slowly inject the sodium borohydride aqueous solution, and terminate the photodeposition reaction after 60 minutes, during which the room temperature is maintained in a constant temperature water bath; after the reaction, the sample is centrifuged, washed with ultrapure water and anhydrous ethanol to remove residual salt, and dried in a vacuum oven at 60°C for 12 hours to obtain Cu-ZnIn2S4 material.

[0039] The XRD patterns of the Cu-ZIS / CNTs composite material, ZnIn2S4 material and Cu-ZnIn2S4 material prepared in Example 1 are shown in Figure 1 As shown in the figure, the prepared Cu-ZnIn2S4 material has obvious characteristic diffraction peak of ZnIn2S4. Due to the low loading amount of Cu, its characteristic diffraction peak is not obvious. The Cu-ZIS / CNTs composite material still has the characteristic diffraction peak of ZnIn2S4, and a weak characteristic peak of CNTs can be observed at about 25°, indicating that Cu, ZnIn2S4 and CNTs have been successfully composited.

[0040] The N2 physical adsorption-desorption curves of the Cu-ZIS / CNTs composite material and ZnIn2S4 material prepared in Example 1 are shown in FIG. Figure 2 As shown, from Figure 2 It can be seen that the adsorption isotherms of the Cu-ZIS / CNTs composite material and the ZnIn2S4 material prepared in Example 1 are both type IV, and the hysteresis loop is H3, indicating that the materials are mesoporous structures. The specific surface area of ​​the ZnIn2S4 material is 84m 2 / g, while the Cu-ZIS / CNTs composite material reaches 123m 2 / g. The specific surface area and pore structure of the composite functional material have changed effectively, which is beneficial to the adsorption and interception of harmful bacteria.

[0041] The TEM image of the Cu-ZIS / CNTs composite material prepared in Example 1 is as follows: Figure 3 As shown, from Figure 3 It can be seen that the main structure of the Cu-ZIS / CNTs composite material is a three-dimensional structure assembled by nanolayers, in which trace amounts of CuNPs and CNTs are anchored and embedded.

[0042] Example 2

[0043] Application of Cu-ZIS / CNTs composites in water disinfection and killing of Pseudomonas aeruginosa

[0044] 1) Prepare the concentration to be 10 8 CFU / mL of Pseudomonas aeruginosa suspension, take 20mL of the prepared PBS buffer solution, keep the water pH at 7.4, add 0.04g of the Cu-ZIS / CNTs composite material prepared by Example 1, ultrasonicate for 2min to evenly disperse the catalyst in the solution, then place the mixed solution under mechanical stirring, control the mixed solution at room temperature of 25°C through a constant temperature water bath, add 0.2ml of Pseudomonas aeruginosa suspension, turn on the light source (150w xenon lamp simulates sunlight, and the visible light band is controlled by optical elements to be 420-630nm), and perform multiphase catalytic water disinfection reaction, with a sampling frequency of 20 minutes each time;

[0045] 2) Take the sample in step 1) above, immediately add 9 ml of PBS buffer solution, repeat dilution to the appropriate multiple, take 0.1 ml and evenly apply it on the agar plate, put the agar plate in an incubator, incubate at 37°C for 24 hours, check and count the number of colonies, and the sterilization effect on the Pseudomonas aeruginosa suspension is as follows: Figure 4 As shown, the inactivation rate of Pseudomonas aeruginosa in simulated water was close to 100% in 60 minutes. Figure 5 , in the comparison of the agar plates before and after sterilization of Pseudomonas aeruginosa, there are almost no colonies after sterilization.

[0046] Control experiment: Carry out water disinfection and sterilization experiments under the action of carbon nanotubes, indium zinc sulfide and no material respectively, Pseudomonas aeruginosa is used as the model bacteria, and the operation process is the same as that of Cu-ZIS / CNTs composite materials used in water disinfection and sterilization of Pseudomonas aeruginosa. Figure 4 As shown, under the action of carbon nanotubes and no material, there is no sterilization efficiency of bacteria, and 100% inactivation rate requires 120 minutes under the catalysis of sulfur indium zinc.

[0047] Example 3

[0048] Cu-ZIS / CNTs composite material is highly effective in disinfecting Escherichia coli

[0049] The Cu-ZIS / CNTs composite material used is from Example 1. Referring to the water disinfection process of Example 2, only Escherichia coli is used as the disinfection evaluation object. Figure 5 It can be seen that after 60 minutes, the inactivation rate of Escherichia coli by the Cu-ZIS / CNTs composite material disinfection system can be close to 100%.

[0050] Example 4

[0051] Cu-ZIS / CNTs composite material is highly effective in disinfecting Staphylococcus aureus

[0052] The Cu-ZIS / CNTs composite material used is from Example 1. The water disinfection process of Example 2 is referred to, except that Staphylococcus aureus is used as the disinfection evaluation object. Figure 5 It can be seen that after 60 minutes, the inactivation rate of the Cu-ZIS / CNTs composite disinfection system against Staphylococcus aureus is also close to 100%.

[0053] Example 5

[0054] Repeated stability of Cu-ZIS / CNTs composites in disinfecting Pseudomonas aeruginosa

[0055] After the Pseudomonas aeruginosa disinfecting experiment was completed in Example 2, the centrifugal rate was controlled, the Cu-ZIS / CNTs composite material was recovered, and it was repeatedly rinsed 5 times with ultrapure water and anhydrous ethanol, and ultrasonically dispersed in a PBS buffer solution again. The water disinfection and sterilization test process in Example 2 was implemented, and the sampling point was selected for 60 minutes. Figure 6 It can be found that the inactivation rate after repeated use is still close to 100%.

[0056] Example 6

[0057] After the Pseudomonas aeruginosa disinfecting experiment was completed in Example 5, the Cu-ZIS / CNTs composite material was recovered according to the recovery process of Example 5, and then the experimental process of Example 2 was implemented, and the sampling point was selected for 60 minutes. Figure 6 It can be found that the inactivation rate of flammable substances after repeated use is close to 100%.

[0058] Example 7

[0059] After the Pseudomonas aeruginosa disinfecting experiment was completed in Example 6, the Cu-ZIS / CNTs composite material was recovered according to the recovery process of Example 5, and then the experimental process of Example 2 was implemented, and the sampling point was selected for 60 minutes. Figure 6 It can be found that the inactivation rate of flammable substances after repeated use for three times is close to 100% (the calculated result is 98.2%).

[0060] Example 8

[0061] After the Pseudomonas aeruginosa disinfecting experiment was completed in Example 7, the Cu-ZIS / CNTs composite material was recovered according to the recovery process of Example 5, and then the test process of Example 2 was implemented, and the sampling point was selected for 60 minutes. Figure 6 It can be found that the inactivation rate of flammable substances after repeated use for 4 times is close to 100% (the calculated result is 97%).

[0062] From the results of repeated tests, the Cu-ZIS / CNTs composite material has very good stability. There is a very small reduction with the repeated tests, which may be caused by losses and errors in the material recovery operation.

[0063] Example 9 Preparation of Cu-ZIS / GR composite material and its application in water disinfection and sterilization

[0064] Preparation of Cu-ZIS / GR composites:

[0065] 1) Dissolve 0.068g ZnCl2, 0.239g InCl2·4H2O and 0.15g CH3CSNH2 in water respectively, mix and stir in turn, and stir magnetically for 30min to form 40mL mixed metal salt solution A; adjust the pH of the mixed solution A to 1.0 with 5M HCl solution; then weigh 2mg graphene and add it to solution A, continue stirring for 12h to obtain a mixed solution B; then transfer the mixed solution B to a hydrothermal reactor with a polytetrafluoroethylene liner; seal the hydrothermal reactor and put it in an oven, heat it to 160℃ and keep it for 16h; after the reaction is completed, cool it to room temperature, centrifuge the precipitate, wash it several times with ultrapure water and anhydrous ethanol to obtain a dark yellow solid, place it in a vacuum oven at 60℃ and vacuum dry it for 12h to obtain a three-dimensional nanostructured ZnIn2S4 / GR composite functional material;

[0066] 2) Dissolve 4.2 mg CuCl2 in 5 mL ultrapure water, and ultrasonically prepare a copper ion solution for later use; dissolve 14.3 mg NaBH4 in 5 mL ultrapure water, and ultrasonically prepare a sodium borohydride aqueous solution for later use; ultrasonically disperse 100 mg of the ZnIn2S4 / GR composite material obtained in step 1) in 40 mL of water, and ultrasonically disperse it evenly, mix it with the prepared copper ion solution, and move it into a quartz photoreactor after ultrasonication, and drive away the dissolved oxygen with nitrogen bubbling. Under magnetic stirring and illumination, slowly inject the sodium borohydride aqueous solution, and terminate the photodeposition reaction after 60 minutes, during which the room temperature is maintained in a constant temperature water bath; after the reaction, the sample is centrifuged, washed with ultrapure water and anhydrous ethanol to remove residual salt, and dried in a vacuum oven at 60°C for 12 hours to obtain the non-precious metal copper-based composite material, which is marked as Cu-ZIS / GR composite material.

[0067] Application of Cu-ZIS / GR composite materials in water disinfection and sterilization

[0068] The construction and analysis test process of the water disinfection and sterilization system are the same as those in Example 2, except that the catalyst is replaced by the Cu-ZIS / GR composite material prepared in this case, and the same dosage as in Example 2 is used. After 100 minutes of illumination, the Cu-ZIS / GR composite material can achieve a 100% inactivation rate for Pseudomonas aeruginosa in the simulated water.

[0069] Example 10 Preparation of Cu-ZIS / BC composite material and its application in water disinfection and sterilization

[0070] Preparation of Cu-ZIS / BC composites:

[0071] 1) Dissolve 0.068g ZnCl2, 0.239g InCl2·4H2O and 0.15g CH3CSNH2 in water respectively, mix well in turn, and stir magnetically for 30min to form 40mL mixed metal salt solution A; adjust the pH of the mixed solution A to 1.0 with 5M HCl solution; then weigh 2mg biochar and add it to solution A, continue stirring for 12h to obtain a mixed solution B; then transfer the mixed solution B to a hydrothermal reactor with a polytetrafluoroethylene liner; seal the hydrothermal reactor and put it in an oven, heat it to 160℃ and keep it for 16h; after the reaction is completed, cool it to room temperature, centrifuge the precipitate, wash it several times with ultrapure water and anhydrous ethanol to obtain a dark yellow solid, place it in a vacuum oven at 60℃ and vacuum dry it for 12h to obtain a three-dimensional nanostructured ZnIn2S4 / BC composite functional material;

[0072] 2) Dissolve 4.2 mg CuCl2 in 5 mL ultrapure water, and ultrasonically prepare a copper ion solution for later use; dissolve 14.3 mg NaBH4 in 5 mL ultrapure water, and ultrasonically prepare a sodium borohydride aqueous solution for later use; ultrasonically disperse 100 mg of the ZnIn2S4 / GR composite material prepared in step 1) in 40 mL of water, and ultrasonically disperse it evenly, mix it with the prepared copper ion solution, and move it into a quartz photoreactor after ultrasonic treatment, and drive away the dissolved oxygen with nitrogen bubbling. Under magnetic stirring and illumination, slowly inject the sodium borohydride aqueous solution, and terminate the photodeposition reaction after 60 minutes, during which the room temperature is maintained in a constant temperature water bath; after the reaction, the sample is centrifuged, washed with ultrapure water and anhydrous ethanol to remove residual salt, and dried in a vacuum oven at 60°C for 12 hours to obtain the non-precious metal copper-based composite material, which is marked as Cu-ZIS / BC composite material.

[0073] Application of Cu-ZIS / BC composite materials in water disinfection and sterilization

[0074] The construction and analysis test process of the water disinfection and sterilization system are the same as those in Example 2, except that the catalyst is replaced by the Cu-ZIS / BC composite material prepared in this case, and the same dosage as in Example 2 is used. After 100 minutes of illumination, the Cu-ZIS / BC composite material can achieve a 98% inactivation rate for Pseudomonas aeruginosa in the simulated water.

[0075] Embodiment 11

[0076] Preparation of Cu-ZIS / CNTs composites under different pH conditions:

[0077] The preparation process of the composite material is the same as that of Example 1, except that the pH value of the solution is adjusted in step 1) to 0.5, 2.5, and 5.0. When the pH is 0.5-5, the overall morphology of the synthesized material is mainly a three-dimensional flower ball self-assembled by nanosheets, but as the pH increases, the surface of the microsphere gradually collapses slightly.

[0078] Example 12

[0079] Preparation of Cu-ZIS / CNTs composites under different reaction time conditions:

[0080] The preparation process of the composite material is the same as that of Example 1, except that the time for placing the hydrothermal reactor in the oven for reaction in step 1) is changed to 6h, 16h, and 48h, respectively. When the reaction time is 6-48h, the overall morphology of the synthesized material does not change significantly.

[0081] Embodiment 13

[0082] Preparation of Cu-ZIS / CNTs composites under different reaction temperature conditions:

[0083] The preparation process of the composite material is the same as that of Example 1, except that the temperature of the hydrothermal reactor in the oven in step 1) is changed to 100°C, 160°C, and 220°C, respectively. When the temperature is 100-220°C, the overall morphology of the synthesized material does not change significantly, but when the reaction temperature is lower, the size difference of the synthesized material is more obvious.

[0084] Embodiment 14

[0085] Preparation of Cu-ZIS / CNTs composites with different metal salts for water sterilization and disinfection:

[0086] The preparation process of the composite material is the same as that of Example 1, except that the types of zinc salt, indium salt, sulfur source and copper salt in step 1) and step 2) are changed. The types of the selected salts are shown in Table 1.

[0087] Table 1 Summary of bactericidal properties of composite materials prepared from different metal salts

[0088]

[0089] The construction and analysis and testing process of the water disinfection and sterilization system is the same as that of Example 2, except that the catalyst is replaced by the Cu-ZIS / CNTs composite material prepared by different metal salts in this case, and the same dosage as in Example 2 is used. The Cu-ZIS / CNTs composite material in this case is used for water disinfection and sterilization, and the sterilization and disinfection effect on Pseudomonas aeruginosa is shown in Table 1. It can be seen from Table 1 that after 100 minutes of illumination, the Cu-ZIS / CNTs composite material synthesized by different metal salts has an inactivation rate of more than 95% on Pseudomonas aeruginosa in the simulated water.

Claims

1. A method for preparing a copper-modified non-precious metal carbon-based composite material, characterized in that: The steps include: 1) Dissolve the zinc salt, indium salt and sulfur source in water respectively, mix them in turn, stir them magnetically to obtain a mixed solution, adjust the pH of the mixed solution to 0.5-5, introduce the carbon-based material, continue stirring, and after stirring, transfer the mixed solution to a hydrothermal reactor and move it to an oven for reaction; 2) After the reaction is completed, the reaction is cooled to room temperature, the precipitate is centrifuged and washed with ultrapure water and anhydrous ethanol to obtain a dark yellow solid, which is then placed in a vacuum oven and dried overnight to obtain a sulfur-indium-zinc / carbon-based composite material; 3) dissolving the copper salt in ultrapure water, ultrasonically preparing a copper ion solution for later use, ultrasonically dispersing the sulfur indium zinc / carbon-based composite material prepared in step 2) in water, mixing it with the prepared copper ion solution, and transferring it into a photoreactor after ultrasonic treatment, bubbling nitrogen to remove dissolved oxygen, and slowly injecting a reducing solution under magnetic stirring and light irradiation, and performing a photodeposition reaction for 5-180 minutes to obtain a nano-copper-modified sulfur indium zinc / carbon-based composite material; 4) centrifugally separating the nano-copper modified sulfur indium zinc / carbon-based composite material prepared in step 3), washing with ultrapure water and anhydrous ethanol to remove residual salt, and drying in a vacuum oven overnight to obtain a copper-modified non-precious metal carbon-based composite material; The carbon-based material in step 1) is one or a mixture of carbon nanotubes, graphene and biochar, and the amount of the carbon-based material added is 0.1-10% of the mass of sulfur indium zinc; The reducing solution in step 3) is hydrazine, sodium borohydride, potassium borohydride, ethanol, ammonia water or sodium sulfite, the concentration of the reducing solution is 0.01-0.6 mol / L, the molar ratio with the copper salt is 3-15:1, and the injection speed of the reducing solution is 2-3 drops / second.

2. The method for preparing a copper-modified non-precious metal carbon-based composite material according to claim 1, characterized in that The zinc salt in step 1) is zinc chloride, zinc nitrate, zinc sulfate, zinc phosphate, zinc acetate, zinc citrate, zinc isooctanoate or zinc glycinate, the indium salt is indium chloride, indium nitrate, indium sulfate, indium phosphate, indium acetate or indium citrate, and the sulfur source is thioacetamide, ammonium sulfide, thiourea or sodium thiosulfate.

3. A method for preparing a copper-modified non-precious metal carbon-based composite material as described in any one of claims 1-2, characterized in that The molar ratio of the zinc salt, indium salt and sulfur source in step 1) is 1-1.5:2-3:4-6.

4. The method for preparing a copper-modified non-precious metal carbon-based composite material according to claim 3, characterized in that The copper salt in step 3) is copper chloride, copper nitrate, copper phosphate, copper acetate or sodium copper ethylenediaminetetraacetate, and the amount of copper salt added is 0.5-20% of the mass of the sulfur indium zinc / carbon-based composite material.

5. The method for preparing a copper-modified non-precious metal carbon-based composite material according to claim 1, characterized in that In step 1), the carbon-based material is introduced and stirring is continued for 1-24 hours. The reaction temperature in the oven is 100-220° C. and the reaction time is 6-48 hours.

6. A copper-modified non-precious metal carbon-based composite material prepared by the preparation method as claimed in claim 5.

7. An application of the copper-modified non-precious metal carbon-based composite material as claimed in claim 6, characterized in that The copper-modified non-precious metal carbon-based composite material is placed in a water body containing harmful bacteria. Under visible light irradiation, a constant temperature water bath is used to maintain the water temperature at room temperature, and PBS buffer is used to maintain the water pH at 7.

4. The pathogens in the water body are disinfected by multiphase catalysis. After the disinfection reaction is completed, the non-precious metal copper-based composite material is separated and recovered.

Citation Information

Patent Citations

  • Preparation method and application of ZnIn2S4-graphene composited photochemical catalyst

    CN102407147A

  • Composite photocatalyst MxP / indium zinc sulfide as well as preparation method and application thereof

    CN108620105A

  • Metallic nickel modified sulfur-indium-zinc photocatalyst and preparation method and application thereof

    CN111013608A