A granite-based mineral admixture and its preparation method and application

Through the crushing, filtering, ball milling and chemical modification of granite cutting tailings, a highly active granite-based mineral admixture is formed, which solves the problem in the existing technology that granite cannot fully exert its chemical effect in concrete and realizes Preparation of high-strength concrete and efficient use of resources.

CN116102278BActive Publication Date: 2024-10-25ANHUI ZHONGTIE ENGINEER MATERIAL SCI & TECH CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310160456.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-10-25
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively utilize granite cutting tailings, fails to fully exert its chemical role in concrete, and is costly, making it difficult to achieve large-scale consumption and preparation of high-strength concrete.

Method used

By crushing, filtering, ball milling and chemically modifying the granite cutting tailings, the steel pickling waste liquid is used to partially dissolve the surface of the granite particles to generate chemical components that participate in the cement hydration reaction, and anhydrous is added during the grinding process. Gypsum is used to reduce the moisture content and increase the particle size to form a highly active granite-based mineral admixture.

Benefits of technology

The mechanical properties of concrete are significantly improved, and the 28-day compressive strength can reach 39.6MPa, realizing high value and resource utilization of granite cutting tailings, and reducing production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a granite-based mineral admixture and a preparation method and application thereof. The preparation method of the granite-based mineral admixture comprises the following steps: (1) granite cutting tailings are subjected to crushing treatment and filter pressing treatment in sequence to obtain granite particles; (2) steel pickling waste liquid and the granite particles obtained in step (1) are mixed by first ball milling to obtain activated granite powder; (3) anhydrous gypsum and the activated granite powder obtained in step (2) are mixed by second ball milling to obtain the granite-based mineral admixture. The present invention crushes, filters, ball mills and chemically modifies the granite cutting tailings to obtain a granite-based mineral admixture with low water content, small particle size and high activity, and further obtains a concrete with high compressive strength, thereby realizing the high value and resource utilization of the granite cutting tailings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building material preparation, and in particular to a granite-based mineral admixture and a preparation method and application thereof. Background Art

[0002] In the process of granite processing and machine-made sand production, a large amount of cutting tailings are usually generated. Cutting tailings are a mixture of stone powder, stone chips and water. They are difficult to handle and have a huge stock. At present, they can only be collected and piled up for treatment, which has an adverse impact on the ecological environment and causes a waste of land resources. If stone cutting tailings are used as mineral admixtures for concrete, it can not only provide a wide range of mineral admixtures for the concrete industry, but also solve the environmental problems caused by the accumulation of stone cutting tailings. However, the chemical composition of granite is stable. It does not participate in the hydration reaction when added to concrete, and its chemical composition cannot be dissolved. Therefore, granite generally plays a physical filling role in concrete.

[0003] CN 113402231A discloses a method for producing ready-mixed concrete using stone sawdust, wherein the sawdust stored in a yard is pre-treated to remove stones and debris in the sawdust. Then, sawdust particles with a water content of 20-35%, a methylene blue value of less than 1.0, a sand content of 15-25%, and a powder content of 40-65% are selected, and the sawdust particles are used to replace fly ash and part of the fine sand, and part or all of the fly ash is replaced in the mix, and the rest is used to replace part of the sand, so as to produce concrete of various grades that meet the requirements. However, this method directly uses sawdust particles as mineral admixtures and sand, which only plays a physical filling role, and fails to fully exert its chemical effect in concrete, making it difficult to prepare high-strength concrete.

[0004] CN 104844081A discloses a concrete with granite powder as the main mineral admixture, wherein the raw material ratio of the concrete is: 161-215 parts by weight of water, 234 parts by weight of cement, 730-752 parts by weight of natural sand, 1095-1127 parts by weight of crushed stone, 18-63 parts by weight of granite powder, 108-63 parts by weight of fly ash, 0-3.6 parts by weight of admixture, and the total weight of granite powder and fly ash is 126 parts. The method uses granite powder and fly ash as admixtures to obtain concrete that meets the strength requirements, but the maximum amount of granite powder in the total raw materials is only 17.5%, and the purpose of large-scale consumption cannot be achieved.

[0005] CN 106396453A discloses a modified granite powder admixture and a preparation method thereof. The modified granite powder admixture comprises raw materials including granite powder, inorganic modifier and grinding aid in percentage by weight, wherein the mass ratio of granite powder to inorganic modifier is: 80-85 parts of granite powder, 15-20 parts of inorganic modifier, the mass of the two being 100 parts in total, and the mass of grinding aid accounts for 0.1-0.3% of the sum of the mass of granite powder and inorganic modifier. The invention introduces a modifier to prepare the modified granite powder admixture, but the preparation process of the modifier is complicated, and it needs to consume more oxide raw materials, resulting in high cost.

[0006] In view of the shortcomings of the existing technology, it is necessary to provide a method that can absorb a large amount of granite cutting tailings, has low cost and produces a mineral admixture with high activity. Summary of the invention

[0007] The purpose of the present invention is to provide a granite-based mineral admixture and a preparation method and application thereof. By crushing, filtering, ball milling and chemically modifying the granite cutting tailings, the effective chemical components in the granite are partially dissolved to form a chemical additive that can promote cement hydration. At the same time, the physical filling effect of the granite powder is utilized to use the obtained highly active granite-based mineral in concrete, which can significantly improve its mechanical properties.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing a granite-based mineral admixture, the preparation method comprising the following steps:

[0010] (1) Granite cutting tailings are successively crushed and filtered to obtain granite particles;

[0011] (2) first ball milling the steel pickling waste liquid and the granite particles obtained in step (1) to obtain activated granite powder;

[0012] (3) A second ball mill is performed to mix anhydrous gypsum and the activated granite powder obtained in step (2) to obtain the granite-based mineral admixture.

[0013] The present invention firstly crushes the granite cutting tailings to obtain fine particle slurry, which can not only improve the efficiency of the next step of ball milling, but also prevent the large granite cutting tailings from clogging the tailings sludge filter press pipeline; then the water content of the granite fine particles is reduced by filter pressing, which can replace the step of drying the granite fine particles and reduce the production cost; further, the granite powder with a smaller particle size can be obtained by ball milling, thereby improving the physical filling effect of the granite powder in concrete; the steel pickling waste liquid is used for mixing and grinding, so that the surface of the granite particles is partially dissolved, and the chemical components participating in or promoting the cement hydration reaction are generated, thereby improving the chemical activity of the granite, and the surface of the granite powder can be made rough and uneven, so that the overlap with the cement hydration product is more firm, and the cement stone structure formed is more compact; anhydrous gypsum is added during the grinding process, which can react chemically with the water in the granite particles and reduce its water content. The above-mentioned partially dissolved chemical components, the steel pickling waste liquid that is not completely reacted, and the generated dihydrate gypsum all participate in or promote the cement hydration reaction, making the granite-based mineral admixture a highly active mineral admixture, which greatly promotes its application in concrete.

[0014] Preferably, the rotation speed of the crushing process in step (1) is 2330-2350 r / min, for example, it can be 2330 r / min, 2335 r / min, 2340 r / min, 2345 r / min or 2350 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0015] Preferably, the power of the crushing process in step (1) is 3kw.

[0016] Preferably, the filtration treatment in step (1) is carried out in a tailings sludge filter press.

[0017] Preferably, the average particle size of the granite particles in step (1) is 80-100 mesh, for example, 80 mesh, 85 mesh, 90 mesh, 95 mesh or 100 mesh, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] Preferably, the moisture content of the granite particles in step (1) is less than 5%, for example, it can be 4.9%, 4.5%, 4%, 3% or 2%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] Preferably, the mass ratio of the granite particles to the steel pickling waste liquid in step (2) is (95-105):1, for example, it can be 95:1, 98:1, 100:1, 102:1 or 105:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the acid in the steel pickling waste liquid in step (2) includes nitric acid and hydrofluoric acid.

[0021] Preferably, the mass concentration of acid in the steel pickling wastewater in step (2) is 8-12%, for example, it can be 8%, 9%, 10%, 11% or 12%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] The steel pickling wastewater mainly contains H + 、F - 、NO3 - , Fe 2+ Cr 3+ 、Ni 2+ Plasma, while the main components of granite are potassium feldspar, sodium feldspar, quartz, mica, etc., by ball milling the low-water content granite fine particles with steel pickling waste liquid, the hydrofluoric acid in the steel pickling waste liquid first reacts chemically with the granite, the process is as follows:

[0023] SiO2+HF→SiF4↑+H2O

[0024] NaAlSi3O8+HF→Na2SiF6+Al2(SiF6)3

[0025] KAlSi3O8+HF→K2SiF6+Al2(SiF6)3

[0026] Na2SiF6, Al2(SiF6)3, K2SiF6 obtained by chemical reaction and NO3 in steel pickling wastewater - , Fe 2+ They can all participate in or promote the hydration reaction of cement, generate more cement hydration products, and thus increase the strength and density of concrete.

[0027] Preferably, the rotation speed of the first ball milling mixing in step (2) is 55-65 r / min, for example, it can be 55 r / min, 58 r / min, 60 r / min, 62 r / min or 65 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] Preferably, the first ball milling mixing time in step (2) is 0.9-1.1 h, for example, 0.9 h, 0.95 h, 1 h, 1.05 h or 1.1 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, the power of the first ball milling mixing in step (2) is 3kw.

[0030] Preferably, the molar ratio of the anhydrous gypsum to the water in the activated granite powder in step (3) is (0.4-0.6):1, for example, it can be 0.4:1, 0.45:1, 0.5:1, 0.55:1 or 0.6:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] After the initial crushing, filtration, ball milling and steel pickling waste liquid treatment, the moisture content of granite particles is still higher than 1%, and the particles are easy to agglomerate, which is not conducive to transportation. Adding anhydrous gypsum during the ball milling process can produce a chemical reaction with the water in the granite particles to generate dihydrate gypsum, reducing the moisture content of the granite particles to less than 1%; in addition, the generated dihydrate gypsum can participate in the cement hydration reaction, produce more calcium aluminate crystals, and increase the strength of concrete.

[0032] Preferably, the rotation speed of the second ball milling mixing in step (3) is 75-85 r / min, for example, it can be 75 r / min, 78 r / min, 80 r / min, 82 r / min or 85 r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the second ball milling mixing time in step (3) is 0.9-1.1 h, for example, 0.9 h, 0.95 h, 1 h, 1.05 h or 1.1 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] As a preferred technical solution of the preparation method described in the first aspect of the present invention, the preparation method comprises the following steps:

[0035] (1) The granite cutting tailings are crushed at a power of 3 kW and a rotation speed of 2330-2350 r / min, and then filtered in a tailings sludge filter press to obtain granite particles with an average particle size of 80-100 mesh and a moisture content of less than 5%;

[0036] (2) mixing the granite particles obtained in step (1) with steel pickling waste liquid at a mass ratio of (95-105):1 at a power of 3 kW and a rotation speed of 55-65 r / min for 0.9-1.1 h to obtain activated granite powder; the acid in the steel pickling waste liquid includes nitric acid and hydrofluoric acid; the mass concentration of the acid in the steel pickling waste liquid is 8-12%;

[0037] (3) mixing the anhydrous gypsum and the activated granite powder obtained in step (2) by a second ball mill at 75-85 r / min for 0.9-1.1 h to obtain the granite-based mineral admixture; the molar ratio of water in the anhydrous gypsum to the activated granite powder is (0.4-0.6):1.

[0038] In a second aspect, the present invention provides a granite-based mineral admixture, wherein the granite-based mineral admixture is prepared by the preparation method described in the first aspect.

[0039] The average particle size of the granite-based mineral admixture is 800-1250 mesh, for example, it can be 800 mesh, 900 mesh, 1000 mesh, 1100 mesh or 1250 mesh, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] The moisture content of the granite-based mineral admixture is less than 1%, for example, it can be 0.9%, 0.7%, 0.5%, 0.3% or 0.1%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] In a third aspect, the present invention provides a use of the granite-based mineral admixture as described in the second aspect, wherein the granite-based mineral admixture is used to prepare concrete.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The preparation method provided by the present invention partially dissolves the effective chemical components in the granite by crushing, filtering, ball milling and chemically modifying the granite cutting tailings, thereby forming a chemical additive that can promote cement hydration, and at the same time improves the surface roughness of the granite powder, and the overlap with the cement hydration product is more firm. The prepared granite-based mineral admixture has low moisture content, small particle size and high activity. Combined with the physical filling effect of the granite-based mineral admixture, the prepared concrete has a 28d compressive strength of up to 39.6MPa, thereby realizing the high value and resource utilization of the granite cutting tailings. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0045] Example 1

[0046] This embodiment provides a granite-based mineral admixture, and the preparation method of the granite-based mineral admixture comprises the following steps:

[0047] (1) The granite cutting tailings were crushed in a tailings sludge filter press at a power of 3 kW and a rotation speed of 2330 r / min, and then filtered to obtain granite particles with an average particle size of 80 mesh and a moisture content of 3.6%;

[0048] (2) mixing the granite particles obtained in step (1) with steel pickling waste liquid at a mass ratio of 100:1 by the first ball mill at a power of 3 kW and a rotation speed of 60 r / min for 1 hour to obtain activated granite powder; the acid in the steel pickling waste liquid includes nitric acid and hydrofluoric acid; the mass concentration of the acid in the steel pickling waste liquid is 10%;

[0049] (3) The anhydrous gypsum and the activated granite powder obtained in step (2) are mixed by a second ball mill at 80 r / min for 1 h to obtain a granite-based mineral admixture with an average particle size of 800 mesh and a water content of 0.2%; the molar ratio of water in the anhydrous gypsum to the activated granite powder is 0.5:1.

[0050] Example 2

[0051] This embodiment provides a granite-based mineral admixture, and the preparation method of the granite-based mineral admixture comprises the following steps:

[0052] (1) The granite cutting tailings were crushed at a power of 3 kW and a rotation speed of 2350 r / min, and then filtered in a tailings sludge filter press to obtain granite particles with an average particle size of 100 mesh and a moisture content of 4.2%;

[0053] (2) mixing the granite particles obtained in step (1) with the steel pickling waste liquid at a mass ratio of 95:1 by the first ball mill at a power of 3 kW and a rotation speed of 65 r / min for 0.9 h to obtain activated granite powder; the acid in the steel pickling waste liquid includes nitric acid and hydrofluoric acid; the mass concentration of the acid in the steel pickling waste liquid is 12%;

[0054] (3) The anhydrous gypsum and the activated granite powder obtained in step (2) are mixed by a second ball mill at 85 r / min for 0.9 h to obtain a granite-based mineral admixture with an average particle size of 1250 mesh and a water content of 0.3%; the molar ratio of water in the anhydrous gypsum to the activated granite powder is 0.4:1.

[0055] Example 3

[0056] This embodiment provides a granite-based mineral admixture, and the preparation method of the granite-based mineral admixture comprises the following steps:

[0057] (1) The granite cutting tailings were crushed in a tailings sludge filter press at a power of 3 kW and a rotation speed of 2340 r / min, and then filtered to obtain granite particles with an average particle size of 90 mesh and a moisture content of 4.5%;

[0058] (2) mixing the granite particles obtained in step (1) with the steel pickling waste liquid at a mass ratio of 105:1 by the first ball mill at a power of 3 kW and a rotation speed of 55 r / min for 1.1 h to obtain activated granite powder; the acid in the steel pickling waste liquid includes nitric acid and hydrofluoric acid; the mass concentration of the acid in the steel pickling waste liquid is 8%;

[0059] (3) The anhydrous gypsum and the activated granite powder obtained in step (2) were mixed by a second ball mill at 75 r / min for 1.1 h to obtain a granite-based mineral admixture with an average particle size of 1000 mesh and a water content of 0.5%; the molar ratio of water in the anhydrous gypsum to the activated granite powder was 0.6:1.

[0060] Example 4

[0061] This embodiment provides a granite-based mineral admixture. The difference between the preparation method of the granite-based mineral admixture and that of Embodiment 1 is that, except for adjusting the mass ratio of the granite particles to the steel pickling waste liquid in step (2) to 90:1, the rest is the same as that of Embodiment 1.

[0062] Example 5

[0063] This embodiment provides a granite-based mineral admixture. The difference between the preparation method of the granite-based mineral admixture and that of Example 1 is that, except for adjusting the mass ratio of the granite particles to the steel pickling waste liquid in step (2) to 110:1, the rest is the same as that of Example 1.

[0064] Example 6

[0065] This embodiment provides a granite-based mineral admixture. The difference between the preparation method of the granite-based mineral admixture and that of Embodiment 1 is that, except for adjusting the molar ratio of the anhydrous gypsum to the water in the activated granite powder in step (3) to 0.3:1, the rest is the same as that of Embodiment 1.

[0066] Example 7

[0067] This embodiment provides a granite-based mineral admixture. The difference between the preparation method of the granite-based mineral admixture and that of Embodiment 1 is that, except for adjusting the molar ratio of the anhydrous gypsum to the water in the activated granite powder in step (3) to 0.8:1, the rest is the same as that of Embodiment 1.

[0068] Comparative Example 1

[0069] This comparative example provides a granite-based mineral admixture. The difference between the preparation method of the granite-based mineral admixture and that of Example 1 is that the mass of the steel pickling waste liquid in step (2) is replaced by single nitric acid, and the rest is the same as that of Example 1.

[0070] Comparative Example 2

[0071] This comparative example provides a granite-based mineral admixture. The difference between the preparation method of the granite-based mineral admixture and that of Example 1 is that in step (2), no steel pickling waste liquid is added to the first ball milling mixing, and the rest is the same as that of Example 1.

[0072] Comparative Example 3

[0073] This comparative example provides a granite-based mineral admixture. The difference between the preparation method of the granite-based mineral admixture and that of Example 1 is that no anhydrous gypsum is added in the second ball milling mixing in step (3), and the rest is the same as that of Example 1.

[0074] The granite-based mineral admixtures provided in Examples 1-7 and Comparative Examples 1-3 were used to prepare concrete according to the components and weight proportions of the concrete in Table 1. The resulting concrete was tested for 28d compressive strength according to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", and the results are shown in Table 2.

[0075] Table 1

[0076] Portland cement Granite-based mineral admixtures medium coarse river sand 5-31.5 stones Water reducing agent water 343 96 752 1039 4.8 164

[0077] Table 2

[0078] 28d compressive strength (MPa) Example 1 37.1 Example 2 39.6 Example 3 38.5 Example 4 31.4 Example 5 33.2 Example 6 35.0 Example 7 33.6 Comparative Example 1 26.5 Comparative Example 2 22.9 Comparative Example 3 24.8

[0079] It can be seen from Table 2 that the granite-based mineral admixture provided by the present invention is treated by ball milling dissolution activation of steel pickling wastewater and ball milling water absorption activation of sufficient anhydrous gypsum, and the moisture content is reduced to within the standard index. The 28d compressive strength of the prepared concrete is close to that of the concrete prepared by using Class II fly ash instead of the granite-based mineral admixture, which meets the standard requirements;

[0080] By comparing Example 1 with Examples 4, 5 and Comparative Example 2, it can be seen that if the steel pickling liquid is too little in the first ball milling mixture, the dissolution and activation effect of the granite particles will decrease, thereby reducing the compressive strength of the concrete; if the steel pickling liquid is too much, the compressive strength of the concrete will also be reduced to a certain extent; by comparing Example 1 with Examples 6, 7 and Comparative Example 3, it can be seen that if the amount of anhydrous gypsum is too little, the water content of the activated granite powder cannot be effectively reduced, resulting in excessive water content, and the 28d compressive strength of the prepared concrete is reduced. If the amount is too much, the compressive strength of the concrete will also be reduced.

[0081] From the comparison between Example 1 and Comparative Example 1, it can be seen that the use of a single nitric acid to activate and dissolve granite particles cannot produce an effective chemical reaction with the mineral components in the granite, further reducing the activation effect and causing a decrease in the compressive strength of the concrete.

[0082] In summary, the preparation method provided by the present invention, by crushing, filtering, ball milling and chemically modifying the granite cutting tailings, partially dissolves the effective chemical components in the granite, forms a chemical additive that can promote cement hydration, and at the same time improves the surface roughness of the granite powder, and makes the overlap with the cement hydration product more firm. The prepared granite-based mineral admixture has low water content, small particle size and high activity. Combined with the physical filling effect of the granite-based mineral admixture, the prepared concrete has a 28d compressive strength of up to 39.6MPa, realizing the high value and resource utilization of the granite cutting tailings.

[0083] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a granite-based mineral admixture, characterized in that: The preparation method comprises the following steps: (1) The granite cutting tailings are crushed at a speed of 2330-2350 r / min and filtered in a tailings sludge filter press to obtain granite particles with an average particle size of 80-100 mesh and a moisture content of less than 5%; (2) the granite particles obtained in step (1) are mixed with steel pickling waste liquid at a mass ratio of (95-105):1 at 55-65 r / min for 0.9-1.1 h to obtain activated granite powder; the acid in the steel pickling waste liquid includes nitric acid and hydrofluoric acid; the mass concentration of the acid in the steel pickling waste liquid is 8-12%; (3) A second ball mill is performed at 75-85 r / min to mix the anhydrous gypsum and the activated granite powder obtained in step (2) 0.9-1.1h, to obtain the granite-based mineral admixture; the molar ratio of the anhydrous gypsum to the water in the activated granite powder is (0.4-0.6):

1.

2. A granite-based mineral admixture, characterized in that: The granite-based mineral admixture is prepared by the preparation method according to claim 1; The average particle size of the granite-based mineral admixture is 800-1250 mesh; The water content of the granite-based mineral admixture is less than 1%.

3. An application of the granite-based mineral admixture as claimed in claim 2, characterized in that: The granite-based mineral admixture is used for preparing concrete.