Pre-coated fin material
By using a resin coating film of modified polyvinyl alcohol and acrylamide polymer on the heat exchanger fin material, the problem of reduced hydrophilicity caused by condensation water and oily contamination is solved, and the hydrophilicity and repellency of the fin surface are achieved. Long-term maintenance of oiliness and removal of pollutants improves heat exchange efficiency.
Patent Information
- Application Number
- CN202180056562.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-13
- Filing Date
- 2021-08-04
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-08-04
AI Technical Summary
During the use of existing heat exchanger fin materials, the reduction in hydrophilicity caused by condensation water and the adhesion of oily pollutants lead to a decrease in heat exchange efficiency, making it difficult to maintain excellent hydrophilicity and remove pollutants for a long time.
A resin coating film containing modified polyvinyl alcohol and acrylamide polymer is used. By adjusting its mass ratio and structure, an excellent hydrophilic and oil-repellent layer is formed to maintain the hydrophilicity of the fin surface for a long time and utilize dew condensation water. Remove attached oily contaminants.
It achieves long-term maintenance of hydrophilicity and oil repellency on the fin surface, improves heat exchange efficiency, can effectively remove oily contaminants, and avoids a decrease in heat exchanger efficiency.
Smart Images

Figure CN116113669B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to pre-coated fin material. Background Art
[0002] As a heat exchanger mounted on an air conditioner, a refrigerator, etc., a so-called cross-fin-tube type heat exchanger is often used, which has a plurality of fins and tubes intersecting these fins. The fins are produced by stamping a pre-coated fin material having a substrate made of aluminum (including pure aluminum and aluminum alloys. The same applies hereinafter) and a resin coating provided on the substrate.
[0003] When the surface temperature of the fins is lower than the dew point of the air during operation of the air conditioner, condensation forms on the fin surfaces, and the gaps between the fins may be clogged by the condensed water. If the gaps between the fins are clogged, the heat exchange efficiency of the heat exchanger may be reduced.
[0004] For this problem, there is a known technology for suppressing the clogging of the gaps between fins caused by condensation water by improving the hydrophilicity of the surface of the fins. For example, Patent Document 1 describes a hydrophilic treatment composition for heat exchanger fin material, which is a hydrophilic treatment composition containing (A) at least one polymer selected from polyglycerol and polyvinyl alcohol, (B) a high acid value acrylic resin having a resin acid value of 300 mgKOH / g or more, and (C) a water-soluble resin other than the above polymer (A) and the high acid value acrylic resin (B), characterized in that the resin solid content of the hydrophilic treatment composition has a resin acid value of 200 mgKOH / g or more and a hydroxyl value of 100 mgKOH / g or more.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2002-38134 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, if condensation water adheres to the surface of the fin during use of the heat exchanger, the hydrophilic substance in the resin coating is washed away by the condensation water, so the hydrophilicity of the fin surface gradually decreases. Furthermore, oily pollutants in the environment such as higher fatty acids and higher alcohols that are present with the use of the heat exchanger adhere to the surface of the fin. These pollutants may cause the hydrophilicity of the fin surface to decrease.
[0010] As described above, conventional fins have problems such as a decrease in hydrophilicity due to condensation water and a gradual decrease in hydrophilicity during use of the heat exchanger due to adhesion of oily contaminants.
[0011] The present invention has been made in view of the above background, and an object of the present invention is to provide a pre-coat fin material which can maintain excellent hydrophilicity for a long period of time and can easily remove oily contaminants adhering to the surface.
[0012] Solutions to Solve Problems
[0013] One embodiment of the present invention is a pre-coated fin material, which has a substrate containing aluminum and a resin coating film formed on the substrate and exposed on the surface, the resin coating film contains a modified polyvinyl alcohol (A) having a molecular structure represented by the following general formula (1) and an acrylamide polymer (B), and the content of the modified polyvinyl alcohol (A) is 0.5 times or more and 2.0 times or less of the content of the acrylamide polymer (B) in terms of mass ratio.
[0014] [Chemistry 1]
[0015]
[0016] Wherein, R in the general formula (1) 1 It is an organic group having a linear structure and having 5 or more and 10 or less carbon atoms, and m and n are positive integers satisfying the relationship of 0.005≤n / m≤0.025.
[0017] Effects of the Invention
[0018] A resin coating film comprising the specific modified polyvinyl alcohol (A) and an acrylamide polymer (B) is provided on the surface of the pre-coated fin material. The resin coating film can improve the hydrophilicity of the surface of the pre-coated fin material and maintain excellent hydrophilicity for a long time by using the specific modified polyvinyl alcohol (A) and making the mass ratio of the modified polyvinyl alcohol (A) to the acrylamide polymer (B) within the specific range.
[0019] In addition, the surface of the pre-coated fin material is not only excellent in hydrophilicity, but also excellent in oil repellency, so it is possible to inhibit oily pollutants from adhering to the surface of the pre-coated fin material. Furthermore, since the pre-coated fin material is excellent in both hydrophilicity and oil repellency, condensation water and the like easily enter between the surface of the pre-coated fin material and the pollutants attached to the surface. Therefore, even if oily pollutants are attached to the surface of the pre-coated fin material, it is possible to use water such as condensation water to wash the pollutants and easily remove them from the surface of the fin.
[0020] As described above, the pre-coated fin material can maintain excellent hydrophilicity for a long period of time and can easily remove oily contaminants attached to the surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1It is a partially enlarged cross-sectional view showing the main parts of test samples 1 to 3 in the examples.
[0022] Figure 2 It is a partially enlarged cross-sectional view showing the main parts of the test samples 4 and 5 in the example. DETAILED DESCRIPTION
[0023] In the precoated fin material, the aluminum constituting the substrate can be appropriately selected from pure aluminum and aluminum alloys according to desired mechanical properties, corrosion resistance, etc. The substrate may be composed of, for example, pure aluminum having a chemical composition represented by alloy numbers such as 1200 and 1050 in JIS H4000.
[0024] A resin coating film containing modified polyvinyl alcohol (A) and acrylamide polymer (B) is formed on a substrate. The resin coating film may be directly laminated on the substrate, or another coating film or coating film may be present between the substrate and the resin coating film.
[0025] For example, the precoated fin material may further include a base coating layered on the substrate. The base coating layer may have effects such as improving the adhesion between the substrate and the corrosion-resistant coating layer and improving the corrosion resistance of the substrate, depending on its material.
[0026] As the base coating, for example, a coating obtained by chemical conversion treatment can be used. As the chemical conversion treatment, for example, chromate treatment using chromate phosphate or the like, and non-chromate treatment using titanium phosphate, zirconium phosphate, molybdenum phosphate, zinc phosphate, zirconium oxide or the like other than chromium compounds can be used.
[0027] It should be noted that the chemical conversion treatment includes reaction-type chemical conversion treatment and coating-type chemical conversion treatment, and the chemical conversion treatment can be carried out by any method. The amount of the base film can be, for example, from 100 mg / m 2 The amount of base coating can be appropriately selected within the following range. The amount of base coating can be measured by a fluorescent X-ray analyzer.
[0028] In addition, the pre-coated fin material may further have a corrosion-resistant coating film between the substrate and the resin coating film. The corrosion-resistant coating film may contain, for example, one or more resins selected from the group consisting of acrylic resins, epoxy resins, polyurethane resins, and ester resins. The corrosion-resistant coating film containing these resins can further improve the corrosion resistance of the fin.
[0029] The film thickness of the corrosion-resistant coating can be appropriately set, for example, within a range of 0.3 μm to 5.0 μm. By setting the film thickness of the corrosion-resistant coating within the specific range, the reduction in heat dissipation performance caused by the corrosion-resistant coating can be avoided, and the effect of improving the corrosion resistance of the fin can be fully obtained.
[0030] The resin coating film provided on the surface of the pre-coated fin material comprises a modified polyvinyl alcohol (A) and an acrylamide polymer (B). The resin coating film may have a hydrophilic layer comprising the modified polyvinyl alcohol (A) and the acrylamide polymer (B). By forming such a hydrophilic layer in the resin coating film, the hydrophilicity and oil repellency of the surface of the pre-coated fin material can be improved, and these properties can be maintained for a long time.
[0031] The film thickness of the resin coating film can be appropriately set, for example, from a range of 0.3 μm or more and 2.0 μm or less. By setting the film thickness of the resin coating film to 0.3 μm or more, the hydrophilicity of the surface of the pre-coated fin material can be improved, and it is easier to remove pollutants attached to the fin surface from the surface of the fin. In addition, by setting the film thickness of the resin coating film to 2.0 μm or less, the coating property of the coating when forming the resin coating film can be improved.
[0032] The modified polyvinyl alcohol (A) in the resin coating film has a molecular structure in which a part of the hydroxyl groups in the polyvinyl alcohol is modified with an organic group having a hydroxyl group at the terminal. Specifically, the modified polyvinyl alcohol (A) has a molecular structure represented by the following general formula (1).
[0033] [Chemistry 2]
[0034]
[0035] Wherein, R in the general formula (1) 1 It is an organic group having a linear structure and having 5 or more and 10 or less carbon atoms, and m and n are positive integers satisfying the relationship of 0.005≤n / m≤0.025.
[0036] The modified polyvinyl alcohol (A) modified by the specific organic group has a bulky organic group introduced into the side chain, so it is not easy to crystallize compared with the unmodified polyvinyl alcohol. Therefore, by mixing the modified polyvinyl alcohol (A) in the resin coating film, the formation of hydrogen bonds can be suppressed, and the hydrophilicity and oil repellency of the surface of the pre-coated fin material can be maintained for a long time.
[0037] From the viewpoint of further improving the above-mentioned effects, R in the general formula (1) 1 An organic group containing a plurality of methylene groups and one or more carbonyl groups is preferred, and an organic group containing a plurality of methylene groups and two or more carbonyl groups is more preferred.
[0038] In the general formula (1), R 1In the case of an organic group containing a carbonyl group, the position of the carbonyl group can be in various forms. For example, the carbonyl group can form an ester bond (-O-CO-) together with the oxygen atom bonded to the main chain of the polyvinyl alcohol. In addition, the carbonyl group can be between methylene groups (-CH2-CO-CH2-). Furthermore, the carbonyl group can form a carboxyl group (-CO-OH) together with the hydroxyl group at the end of the side chain.
[0039] The content of the modified polyvinyl alcohol (A) in the resin coating is more than 0.5 times and less than 2.0 times of the acrylamide polymer (B) in terms of mass ratio. By setting the ratio of the modified polyvinyl alcohol (A) to the acrylamide polymer (B) to the specific range, the hydrophilicity and oil repellency of the surface of the pre-coated fin material can be maintained for a long time. When the ratio of the modified polyvinyl alcohol (A) to the acrylamide polymer (B) is not in the specific range, the resin coating deteriorates earlier in the use of the heat exchanger, which may lead to a reduction in hydrophilicity and oil repellency.
[0040] From the viewpoint of maintaining excellent hydrophilicity and oil repellency for a longer period of time, the content of the modified polyvinyl alcohol (A) is preferably 0.7 times or more and 1.9 times or less, and more preferably 1.0 times or more and 1.6 times or less, that of the acrylamide polymer (B).
[0041] As the acrylamide polymer (B) in the resin coating film, for example, homopolymers such as polyacrylamide and polymethacrylamide using (meth)acrylamide or its derivatives as monomers, copolymers using two or more compounds selected from the group consisting of (meth)acrylamide and its derivatives as monomers, copolymers using one or more compounds selected from the group consisting of (meth)acrylamide and its derivatives and other compounds as monomers, etc. can be used. The resin coating film may contain one or more of these homopolymers and copolymers as the acrylamide polymer (B).
[0042] As acrylamide polymer (B), it is preferred to use a homopolymer of primary amide or secondary amide or a copolymer containing at least one of primary amide and secondary amide as a monomer. These homopolymers and copolymers contain primary amide groups or secondary amide groups with high polarity. Therefore, by using these homopolymers and copolymers as acrylamide polymer (B), the hydrophilicity of the resin coating can be further improved, and pollutants can be removed more easily from the fin surface. From this viewpoint, it is particularly preferred to use polyacrylamide as acrylamide polymer (B).
[0043] The acid value of the acrylamide polymer (B) is preferably 20 mgKOH / g or more and 100 mgKOH / g or less. By using an acrylamide polymer (B) having an acid value in the specific range, excellent hydrophilicity and oil repellency can be maintained for a long time. As a result, pollutants attached to the surface of the fin can be easily removed from the surface of the fin, and the ability to remove pollutants can be maintained for a longer time.
[0044] From the viewpoint of maintaining the ability to remove pollutants for a longer period of time, the acid value of the acrylamide polymer (B) is more preferably 40 mgKOH / g or more. On the other hand, from the viewpoint of further improving the ability to remove pollutants, the acid value of the acrylamide polymer (B) is more preferably 90 mgKOH / g or less.
[0045] In the resin coating, in addition to the modified polyvinyl alcohol (A) and acrylamide polymer (B) as essential components, any component other than these may also be included. When any component is included in the resin coating, the total of the content of the modified polyvinyl alcohol (A) and acrylamide polymer (B) can be appropriately set from the scope of more than 85 mass parts when the mass of the resin coating as a whole is 100 mass parts. In this case, the amount of the modified polyvinyl alcohol (A) and acrylamide polymer (B) in the resin coating can be increased sufficiently. As a result, the effect brought by any component can be obtained while ensuring excellent hydrophilicity and oil repellency.
[0046] The resin coating film may contain polyethylene glycol as an optional component.
[0047] The polyethylene glycol can float on the hydrophilic layer during the formation of the resin coating to form a lubricating layer. The polyethylene glycol exposed on the surface of the resin coating can function as a lubricating material to reduce the friction between the pre-coated fin material and the stamping die when the pre-coated fin material is subjected to stamping, thereby improving the processability during stamping.
[0048] The content of polyethylene glycol in the resin coating is preferably 1.5 parts by mass or more and 8 parts by mass or less relative to 100 parts by mass of the resin coating. By making the content of polyethylene glycol 1.5 parts by mass or more, the friction between the pre-coated fin material and the die during the stamping process can be further reduced. From the viewpoint of further reducing the friction between the pre-coated fin material and the die during the stamping process, the content of polyethylene glycol is preferably 2.0 parts by mass or more, and more preferably 2.5 parts by mass or more.
[0049] In addition, by making the content of polyethylene glycol less than 8 parts by mass, the surface roughness of the pre-coated fin material can be further reduced, making it more difficult for pollutants to adhere to the surface of the fin. From the viewpoint of making the surface of the pre-coated fin material smoother and more effectively inhibiting the adhesion of pollutants to the fin surface, the content of polyethylene glycol is preferably less than 7 parts by mass, and more preferably less than 5 parts by mass.
[0050] The number average molecular weight of the polyethylene glycol is preferably in the range of 1000 to 20000. In this case, lubricity during press working can be improved, and adhesion of contaminants to the fin surface can be more effectively suppressed.
[0051] In the resin coating, as an optional component, a crosslinking agent for making the crystal structure of the modified polyvinyl alcohol (A) more compact may also be included. By adding a crosslinking agent to the resin coating, the hardness of the resin coating can be further improved, and the adhesion of dust can be more effectively suppressed. As the crosslinking agent, for example, melamine resin, blocked isocyanate compounds, etc. can be used. These compounds can be used alone or in combination of two or more.
[0052] In addition, the resin coating film may further contain at least one of an antibacterial agent and a mildewproof agent as an arbitrary component, or both. In addition, an antibacterial / mildewproof agent having both antibacterial and mildewproof effects may be added to the resin coating film. By adding a compound having at least one of an antibacterial and mildewproof effect to the resin coating film, the corrosion of the resin coating film can be suppressed, and the effect produced by the resin coating film can be maintained for a longer period of time.
[0053] As compounds having antibacterial and antifungal effects, for example, organic antibacterial / antifungal agents such as isothiazolin-based antibacterial / antifungal agents, aldehyde-based antibacterial / antifungal agents, benzimidazole-based antibacterial / antifungal agents, halogen-based antibacterial / antifungal agents, carboxylic acid-based antibacterial / antifungal agents, sulfonamide-based antibacterial / antifungal agents, thiazole-based antibacterial / antifungal agents, triazole-based antibacterial / antifungal agents, phenol-based antibacterial / antifungal agents, phthalimide-based antibacterial / antifungal agents, cyclohexane acid-based antibacterial / antifungal agents, and pyridine-based antibacterial / antifungal agents; and inorganic antibacterial / antifungal agents such as Ag, Cu, and Zn can be used.
[0054] As the antibacterial / antifungal agent, at least one of zinc pyrithione, 2,3,5,6-tetrachloro-4-(methylsulfonyl)-pyridine and 2-(4-thiazolyl)benzimidazole is preferably used. These compounds have little effect on the physical properties of the resin coating, are insoluble in water, and have high thermal stability. Therefore, by adding these compounds to the resin coating, the antibacterial and antifungal effects can be maintained for a long time.
[0055] In the resin coating, as an arbitrary component, fluororesin particles containing a fluororesin having a perfluoroalkyl group and having a median particle size of 1 μm or more and 4 μm or less on a volume basis may also be included. At least a portion of the fluororesin particles in the resin coating are arranged on the surface of the hydrophilic layer, and function together with polyethylene glycol as a lubricant during stamping. By making the median particle size of the fluororesin particles within the specific range, the lubricity during stamping can be further reduced. From the viewpoint of more reliably exerting the effect, the content of the fluororesin particles is preferably 2 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the resin coating.
[0056] The volume-based median particle size of the fluororesin particles refers specifically to a particle size at a cumulative 50% in a particle size distribution obtained by a laser diffraction / scattering method.
[0057] As the fluororesin constituting the fluororesin particles, for example, fully fluorinated resins such as polytetrafluoroethylene (i.e., PTFE), partially fluorinated resins such as polyvinylidene fluoride (i.e., PVDF) and polyvinyl fluoride (i.e., PVF), fluorinated resin copolymers such as tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (i.e., PFA) and ethylene-tetrafluoroethylene copolymer (i.e., ETFE) can be used. The fluororesin particles can be composed of particles containing one of these fluororesins, or two or more of them can be used in combination.
[0058] The fluororesin particles are preferably composed of a fluororesin having a perfluoroalkyl group. In this case, the lubricity during the press working can be further improved.
[0059] As a method for producing the pre-coated fin material, for example, the following method can be used: after applying a coating comprising modified polyvinyl alcohol (A) and acrylamide polymer (B) on a substrate, the coating is heated to dry it. In the process of drying the coating, the modified polyvinyl alcohol (A) and the acrylamide polymer (B) settle on the substrate side to form a hydrophilic layer. At this time, the modified polyvinyl alcohol (A) has low compatibility with the acrylamide polymer (B), so in the hydrophilic layer, the phase comprising the modified polyvinyl alcohol (A) and the phase comprising the acrylamide polymer (B) are formed in a state of being separated from each other. On the surface of the hydrophilic layer, the two phases are exposed.
[0060] The phase comprising modified polyvinyl alcohol (A) can show excellent oil repellency derived from modified polyvinyl alcohol (A). And then, in the phase comprising modified polyvinyl alcohol (A), the formation of hydrogen bonds between hydroxyl groups contained in modified polyvinyl alcohol (A) is suppressed by the steric hindrance of the organic group of the imported side chain. Therefore, the hydroxyl groups that do not form hydrogen bonds on the surface of the phase comprising modified polyvinyl alcohol (A) can be exposed more, thereby improving the hydrophilicity of the surface of the hydrophilic layer.
[0061] In addition, the phase containing the acrylamide polymer (B) can exhibit excellent hydrophilicity derived from the acrylamide polymer (B). Therefore, the hydrophilic layer containing the modified polyvinyl alcohol (A) and the acrylamide polymer (B) can have both excellent hydrophilicity and oil repellency.
[0062] The pre-coated fin material is used, for example, in the manufacture of a heat exchanger as described below. First, the pre-coated fin material is cut into the desired size to produce fins. The obtained fins are subjected to slit processing, louver sheet forming, and collar processing in an appropriate combination using a stamping machine to form slits, louver sheets, and collars. Thereafter, a plurality of fins are arranged in a state where they are spaced apart from each other by a specific interval, and a metal tube for circulating the refrigerant is installed in a manner that penetrates these plurality of fins. Thereafter, the outer diameter of the metal tube is expanded by inserting a tube expansion plug into the metal tube, so that the metal tube and the fin are closely fitted. In this way, a heat exchanger can be obtained. The heat exchanger can be assembled into, for example, an indoor unit, an outdoor unit, etc. of an air-conditioning device.
[0063] Example
[0064] Reference Figure 1 The embodiment of the pre-coated fin material is described. Figure 1 As shown, the pre-coated fin material 1 of this example has a substrate 2 containing aluminum and a resin coating film 3 formed on the substrate 2 and exposed on the surface. The resin coating film 3 contains a modified polyvinyl alcohol (A) having a molecular structure represented by the general formula (1) and an acrylamide polymer (B). The content of the modified polyvinyl alcohol (A) is 0.5 times or more and 2.0 times or less of the content of the acrylamide polymer (B) in terms of mass ratio. A more specific example of the pre-coated fin material of this example is described below together with its manufacturing method.
[0065] ·Test material 1 to test material 3
[0066] Test materials 1 to 3 shown in Table 1 can be produced by the following method. First, a substrate 2 is prepared. As the substrate 2, a plate containing aluminum can be used directly, or a plate on which a base coating is formed by chemical conversion treatment in advance can be used. The substrate 2 used in the test materials 1 to 3 is specifically composed of aluminum having a chemical composition represented by alloy number 1050 in JIS H4000, and is a tempered aluminum plate with a thickness of 0.1 mm represented by type number H26 in JIS H0001. The substrate 2 is subjected to a chemical conversion treatment using a chromate phosphate solution in advance, and a base coating 21 composed of chromate phosphate is provided on both surfaces of the substrate 2.
[0067] Next, a coating material containing modified polyvinyl alcohol (A) and acrylamide polymer (B) at the mass ratio shown in Table 1 was prepared. In addition, in Table 1, "polyvinyl alcohol" is abbreviated as "PVA", and "acrylamide polymer" is abbreviated as "PAM".
[0068] The modified polyvinyl alcohol (A) used in Test Materials 1 to 3 has a molecular structure represented by the following structural formula (2).
[0069] [Chemistry 3]
[0070]
[0071] Wherein, R in the structural formula (2) 2 It is an organic group having 7 carbon atoms and a linear structure including both a methylene group and a carbonyl group, and m and n are positive integers satisfying the relationship of 0.005≤n / m≤0.025.
[0072] The acrylamide polymer (B) used in Test Materials 1 to 3 had an acid value of 50 mgKOH / g and a weight average molecular weight of 300,000 in terms of polystyrene.
[0073] After the coating was applied to the substrate 2 using a bar coater, the coating was heated at 225° C. for 10 seconds to dry. Through the above steps, a resin coating film 3 was formed on the substrate 2 to obtain test materials 1 to 3. The thickness of the resin coating film 3 was 1 μm.
[0074] like Figure 1 As shown, the resin coating film 3 of the test samples 1 to 3 has a hydrophilic layer 31 including a phase 311 containing the modified polyvinyl alcohol (A) and a phase 312 containing the acrylamide polymer (B).
[0075] Test material 4 and test material 5
[0076] Test materials 4 and 5 have the same configuration as test materials 1 to 3 except that the resin coating film 3 contains polyethylene glycol. The production method of test materials 4 and 5 is the same as the production method of Examples 1 to 3 except that polyethylene glycol in the amount shown in Table 1 is added to the coating. The number average molecular weight of the polyethylene glycol used in test materials 4 and 5 is 6000. In addition, in Table 1, "polyethylene glycol" is abbreviated as "PEG".
[0077] When the coating material contains polyethylene glycol as in Test Materials 4 and 5, the modified polyvinyl alcohol (A) and acrylamide polymer (B) in the coating material settle toward the substrate 2 during the heating and drying of the coating material on the substrate. Figure 2As shown, a hydrophilic layer 31 including a phase 311 containing a modified polyvinyl alcohol (A) and a phase 312 containing an acrylamide-based polymer (B) was formed on the base film 21 of the test samples 4 and 5.
[0078] On the other hand, polyethylene glycol has a lower viscosity than modified polyvinyl alcohol (A) and acrylamide polymer (B), so it floats to the surface side as the coating dries. Thus, a lubricating layer 32 containing polyethylene glycol is formed on the hydrophilic layer 31. In this way, the resin coating film 302 of the test material 4 and the test material 5 has the lubricating layer 32 exposed on the surface and the hydrophilic layer 31 between the lubricating layer 32 and the substrate 2.
[0079] Test material 6 and test material 7
[0080] Test samples 6 and 7 have the same configuration as test samples 1 to 3 except that the ratio of the modified polyvinyl alcohol (A) to the acrylamide polymer (B) is within the above-mentioned specific range.
[0081] Test material 8
[0082] Test sample 8 has the same configuration as test samples 4 and 5 except that the content of polyethylene glycol is higher than the above-mentioned specific range.
[0083] Test material 9
[0084] Test sample 9 was produced by the same production method as that of test samples 1 to 3, except that unmodified polyvinyl alcohol (number average molecular weight: 6000) was used instead of modified polyvinyl alcohol (A).
[0085] The properties of the test samples 1 to 9 can be evaluated by the following methods.
[0086] Hydrophilicity
[0087] The hydrophilicity of the test material can be evaluated based on the contact angle of water. In this example, the contact angle of water in each test material just after production and the contact angle of water in the test material after the degradation test were measured. The contact angle of water in each test material just after production is shown in Table 1.
[0088] After measuring the contact angle of water just after production, a degradation test was performed. In the degradation test, after the test material was immersed in ion exchange water for 2 minutes, air was blown to each test material for 6 minutes to dry the resin coating 3 and the resin coating 302. This cycle was regarded as 1 cycle, and the cycle was repeated for 300 cycles. Then, water was dripped into the test material after the degradation test was completed, and the contact angle of water was measured. The contact angle of water in the test material after the degradation test is shown in Table 1.
[0089] Oil repellency
[0090] The oil repellency of the test material can be evaluated based on the results of the cleaning test as shown below. First, a square with a side length of 15 mm is drawn on the resin coating film 3 and the resin coating film 302 of the test material using an oil-based dye marker, and the inside of the square is filled with the oil-based dye marker, thereby attaching the ink layer to the resin coating film 3 and the resin coating film 302. It should be noted that as the oil-based dye marker, for example, "Twin Marker MFN-15FB-B" manufactured by Triumph Co., Ltd. can be used.
[0091] Next, the test material was placed vertically, and water was sprayed 150 times using a sprayer on the part of the test material located above the ink layer. At this time, the water sprayed from the sprayer was prevented from directly contacting the square. After the spraying was completed, the area of the ink layer removed by the spraying was measured. Then, the ratio of the area of the ink layer removed by the spraying to the area of the ink layer before the spraying was expressed as a percentage as the removal rate of the ink layer (unit: %)
[0092] The above cleaning test was performed on the test material just after the production and the test material after the degradation test, and the results are shown in the "Oil Repellency" column of Table 1. It should be noted that in the "Oil Repellency" column of Table 1, the removal rate of the ink layer is recorded as "A" when it is higher than 80%, the removal rate is recorded as "B" when it is higher than 60% and less than 80%, the removal rate is recorded as "C" when it is higher than 40% and less than 60%, the removal rate is recorded as "D" when it is higher than 20% and less than 40%, and the removal rate is recorded as "E" when it is less than 20%.
[0093] ·Adhesion
[0094] The adhesion between the substrate 2 and the resin coating 3 or the resin coating 302 can be evaluated by the cross-cutting method specified in JIS K5600-5-6:1999. Specifically, first, the resin coating 3 is cut into a grid shape using a cutting knife, and 100 square pieces with a side length of 2 mm are formed on the resin coating 3 and the resin coating 302. A transparent tape as an attachment tape is pasted on these square pieces. Then, the transparent tape is peeled off at an angle of 45° relative to the substrate 2, and the number of square pieces remaining on the substrate 2 is counted. In the "Adhesion" column of Table 1, the situation where all square pieces remain on the substrate 2 is recorded as "good", and the situation where more than one square piece is peeled off from the substrate 2 is recorded as "bad".
[0095] [Table 1]
[0096]
[0097] As shown in Table 1, test materials 1 to 5 have a resin coating having a composition within the specific range on the substrate. Therefore, the contact angle of water just after the production of these test materials is less than 20°, showing excellent hydrophilicity just after production. In addition, the contact angle of water after the degradation test of these test materials is less than 30°, and high hydrophilicity can be maintained for a long time. Furthermore, these test materials are also excellent in oil repellency just after production and oil repellency after degradation test.
[0098] On the other hand, the mass ratio of the modified polyvinyl alcohol (A) to the acrylamide polymer (B) in Sample 6 was less than the specific range. Therefore, the hydrophilicity and oil repellency of Sample 6 after the degradation test were lower than those of Samples 1 to 5.
[0099] As shown in Table 1, the mass ratio of the modified polyvinyl alcohol (A) to the acrylamide polymer (B) in Test Sample 7 was larger than the specific range. Therefore, the oil repellency of Test Sample 7 after the degradation test was lower than that of Test Samples 1 to 5.
[0100] The content of polyethylene glycol in the test sample 8 was higher than the above-mentioned specific range. Therefore, the adhesion of the resin coating film of the test sample 8 was lower than that of the test samples 1 to 5.
[0101] Since the test material 9 contained unmodified polyvinyl alcohol instead of the modified polyvinyl alcohol (A), the structure of the hydrophilic layer of the test material 9 was different from that of the test materials 1 to 5. The hydrophilicity of the test material 9 after the degradation test was lower than that of the test materials 1 to 5.
[0102] The specific form of the pre-coated fin material according to the present invention is not limited to the form of the embodiment described above, and can be appropriately changed within the scope that does not impair the gist of the present invention. For example, in the embodiment and experimental example described above, an example of the pre-coated fin material 1 in which the base coating 21 is formed on the substrate 2 is shown, but the chemical conversion treatment for forming the base coating 21 can also be omitted, and the resin coating 3 can be directly formed on the substrate 2. In addition, the chemical conversion treatment for forming the base coating 21 can also be omitted, and the corrosion-resistant coating and the resin coating 3 can be formed on the substrate 2 in sequence.
Claims
1. A pre-coated fin material, comprising: A substrate comprising aluminum; and a resin coating film formed on the substrate and exposed on the surface, The resin coating film contains a modified polyvinyl alcohol (A) having a molecular structure represented by the following general formula (1) and an acrylamide polymer (B), The content of the modified polyvinyl alcohol (A) is 0.7 times or more and 2.0 times or less of the content of the acrylamide polymer (B) in terms of mass ratio, In the general formula (1), R 1 is an organic group having a linear structure and having 5 to 10 carbon atoms and containing a plurality of methylene groups and one or more carbonyl groups, wherein m and n are positive integers satisfying the relationship of 0.005≤n / m≤0.025, The acrylamide polymer (B) is polyacrylamide.
2. The precoated fin material according to claim 1, wherein: The resin coating film further contains polyethylene glycol.
3. The precoated fin material according to claim 1 or 2, wherein: The resin coating film further contains one or more compounds selected from the group consisting of blocked isocyanate compounds and melamine resins.
4. The precoated fin material according to claim 1 or 2, wherein: The resin coating film further contains at least one of an antibacterial agent and an antifungal agent.
5. The precoated fin material according to claim 3, wherein: The resin coating film further contains at least one of an antibacterial agent and an antifungal agent.
6. The precoated fin material according to claim 1 or 2, wherein: The resin coating film includes fluororesin particles containing a fluororesin having a perfluoroalkyl group and having a volume-based median particle size of 1 μm or more and 4 μm or less.
7. The precoated fin material according to claim 3, wherein: The resin coating film includes fluororesin particles containing a fluororesin having a perfluoroalkyl group and having a volume-based median particle size of 1 μm or more and 4 μm or less.
8. The precoated fin material according to claim 4, wherein: The resin coating film includes fluororesin particles containing a fluororesin having a perfluoroalkyl group and having a volume-based median particle size of 1 μm or more and 4 μm or less.
9. The precoated fin material according to claim 1 or 2, wherein: The pre-coated fin material has a corrosion-resistant coating film interposed between the substrate and the resin coating film, and the corrosion-resistant coating film contains one or more resins selected from the group consisting of acrylic resins, epoxy resins, and polyurethane resins.
10. The precoated fin material according to claim 3, wherein: The pre-coated fin material has a corrosion-resistant coating film interposed between the substrate and the resin coating film, and the corrosion-resistant coating film contains one or more resins selected from the group consisting of acrylic resins, epoxy resins, and polyurethane resins.
11. The precoated fin material according to claim 4, wherein: The pre-coated fin material has a corrosion-resistant coating film interposed between the substrate and the resin coating film, and the corrosion-resistant coating film contains one or more resins selected from the group consisting of acrylic resins, epoxy resins, and polyurethane resins.
12. The precoated fin material according to claim 6, wherein: The pre-coated fin material has a corrosion-resistant coating film interposed between the substrate and the resin coating film, and the corrosion-resistant coating film contains one or more resins selected from the group consisting of acrylic resins, epoxy resins, and polyurethane resins.
Citation Information
Patent Citations
Hydrophilization treating composition for heat exchanger fin material
JP2002038134A
Precoat fin material
JP2019086267A
Precoat fin material
JP2019100675A