N-type doped single-walled carbon nanotubes and their preparation and application, n-type doped single-walled carbon nanotube thermoelectric film and its preparation method
Through the method of polyvinylpyrrolidone covalent graft modification and organic binder mixing, an n-type doped single-walled carbon nanotube thermoelectric film with high conductivity and flexibility is prepared, which solves the problem of n-type doped single-walled carbon nanotube thermoelectric film in the existing technology. The problem of low mechanical properties of wall carbon nanotube thermoelectric films is suitable for the application of flexible thermoelectric devices.
Patent Information
- Application Number
- CN202211315587.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-10-26
AI Technical Summary
It is difficult to effectively prepare n-type doped single-walled carbon nanotube thermoelectric films with high conductivity using existing technology, and its mechanical properties are low, making it unable to meet the needs of flexible and wearable thermoelectric devices.
Single-walled carbon nanotubes are modified by covalent grafting of polyvinylpyrrolidone to form n-type doped single-walled carbon nanotubes, which are mixed with an organic binder in an organic solvent, and then film-formed and solidified to prepare a n-type doped single-walled carbon nanotube with good flexibility. and uniformity of n-type doped single-walled carbon nanotube thermoelectric films.
It achieves high conductivity and good flexibility, is suitable for the preparation of flexible thermoelectric devices, solves the problem of low mechanical properties of traditional n-type doped single-walled carbon nanotube thermoelectric films, and provides a simple and low-cost preparation method.
Smart Images

Figure CN116119652B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thermoelectric materials, and specifically relates to n-type doped single-walled carbon nanotubes and preparation and application thereof, n-type doped single-walled carbon nanotube thermoelectric films and preparation methods thereof. Background Art
[0002] Thermoelectric devices are devices that can realize the mutual conversion of heat energy and electrical energy. They have two main applications: one is temperature difference power generation; the other is thermoelectric cooling and heating. Thermoelectric materials used in thermoelectric devices are a new type of energy material that is environmentally friendly and has broad application prospects.
[0003] The adjacent carbon atoms of single-walled carbon nanotubes (SWCNTs) form a hexagonal arrangement. Each carbon atom is adjacent to three nearest atoms to form a covalent bond. The remaining electron is called a π electron. The π electron can move almost freely in the carbon tube. The conductivity of single-walled carbon nanotubes mainly depends on the π electron. As a typical one-dimensional material, SWCNTs have attracted widespread attention in the field of thermoelectric materials due to their excellent mechanical, electrical and thermal properties. At present, SWCNTs have been successfully applied to the field of thermoelectric materials. Since SWCNTs composite thermoelectric materials have the advantages of light weight, strong flexibility and low cost, they are more suitable for flexible, stretchable, wearable electronic devices and complex working environments with non-flat surfaces.
[0004] A complete thermoelectric device usually requires both p-type and n-type materials to work simultaneously. Currently, p-type doping of SWCNTs is very simple and requires almost no additional operations, because SWCNTs absorb oxygen from the air and are oxidized by oxygen, causing them to exhibit p-type behavior.
[0005] However, n-type doping of SWCNTs is more challenging than p-type doping. Currently, people often use organic small molecules and polyethyleneimine as electron donors to prepare n-type SWCNTs. However, the film-forming properties of organic small molecules are poor, and the mechanical properties of the prepared SWCNTs films are low. The inherent amplified electrical insulation of polyethyleneimine inevitably leads to a decrease in the conductivity of SWCNTs. Summary of the invention
[0006] The purpose of the present invention is to provide n-type doped single-walled carbon nanotubes and their preparation and application, n-type doped single-walled carbon nanotube thermoelectric film and its preparation method. The n-type doped single-walled carbon nanotubes provided by the present invention have n-type semiconductor characteristics, and the n-type doped single-walled carbon nanotube thermoelectric film has good flexibility and uniformity, and is expected to be prepared with existing p-type thermoelectric films into flexible thermoelectric devices that can be worn by the human body. The preparation method provided by the present invention is simple and safe, and the obtained n-type doped single-walled carbon nanotubes have high electrical conductivity.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The invention provides an n-type doped single-wall carbon nanotube, comprising a single-wall carbon nanotube modified by covalent grafting of polyvinyl pyrrolidone.
[0009] Preferably, the mass ratio of the polyvinyl pyrrolidone to the single-walled carbon nanotubes is (2-4):1.
[0010] The present invention provides a method for preparing n-type doped single-walled carbon nanotubes as described in the above technical solution, comprising the following steps:
[0011] Mixing polyvinyl pyrrolidone, single-walled carbon nanotubes and an alcohol solvent to obtain a suspension;
[0012] In a protective gas atmosphere, the suspension is heated to perform a grafting reaction to obtain the n-type doped single-walled carbon nanotubes.
[0013] Preferably, the temperature of the grafting reaction is 270-280° C., and the insulation time of the grafting reaction is 15-24 hours.
[0014] Preferably, the grafting reaction directly obtains a grafting reaction liquid, and after the grafting reaction, the grafting reaction liquid is subjected to alcohol precipitation, solid-liquid separation and washing in sequence to obtain the n-type doped single-walled carbon nanotubes; the alcohol solvent used for the alcohol precipitation is isopropanol.
[0015] The present invention provides the use of the n-type doped single-walled carbon nanotubes described in the above technical solution or the n-type doped single-walled carbon nanotubes prepared by the preparation method described in the above technical solution as thermoelectric materials.
[0016] The present invention provides a method for preparing an n-type doped single-walled carbon nanotube thermoelectric film, comprising the following steps:
[0017] The n-type doped single-walled carbon nanotubes, an organic binder and an organic solvent are mixed to obtain a mixed slurry; the n-type doped single-walled carbon nanotubes are the n-type doped single-walled carbon nanotubes described in the above technical solution or the n-type doped single-walled carbon nanotubes prepared by the preparation method described in the above technical solution;
[0018] Forming the mixed slurry into a film to obtain a wet film;
[0019] The wet film is heated and cured to obtain the n-type doped single-walled carbon nanotube thermoelectric film.
[0020] Preferably, the organic adhesive comprises polyvinylidene fluoride, and the mass ratio of the n-type doped single-walled carbon nanotubes to the organic adhesive is (4-6):1.
[0021] Preferably, the curing temperature is 75-80° C., and the curing insulation time is 1-3 hours.
[0022] The present invention provides an n-type doped single-walled carbon nanotube thermoelectric film prepared by the preparation method described in the above technical solution, wherein the n-type doped single-walled carbon nanotube thermoelectric film is a self-supporting flexible film.
[0023] The present invention provides an n-type doped single-walled carbon nanotube, including a single-walled carbon nanotube modified by covalent grafting of polyvinyl pyrrolidone. The present invention uses polyvinyl pyrrolidone (PVP) with excellent physiological inertness and excellent biocompatibility as an electron-donating reducing agent. When single-walled carbon nanotubes (SWCNTs) are modified by covalent bond grafting, it can form a CN covalent bond with the free π electrons of SWCNTs to provide electrons for SWCNTs, thereby making SWCNTs have n-type semiconductor characteristics. At the same time, PVP is adsorbed on the surface of SWCNTs through covalent bonds. As a surfactant, it can improve the dispersibility of n-type doped SWCNTs and make the n-type doped SWCNTs more evenly dispersed.
[0024] The present invention provides a method for preparing n-type doped single-walled carbon nanotubes as described in the above technical solution, comprising the following steps: mixing polyvinyl pyrrolidone, single-walled carbon nanotubes and an alcohol solvent to obtain a suspension; heating the suspension in a protective gas atmosphere for a grafting reaction to obtain the n-type doped single-walled carbon nanotubes. The preparation method provided by the present invention uses PVP as an electron-donating reducing agent to covalently graft and modify SWCNTs in an alcohol solution, thereby preparing n-type doped single-walled carbon nanotubes. The preparation method provided by the present invention is simple, low-cost, easy to implement, and is expected to be applied on a large scale.
[0025] The present invention provides a method for preparing an n-type doped single-walled carbon nanotube thermoelectric film, comprising the following steps: mixing the n-type doped single-walled carbon nanotube, an organic adhesive and an organic solvent to obtain a mixed slurry; the n-type doped single-walled carbon nanotube is the n-type doped single-walled carbon nanotube described in the above technical solution or the n-type doped single-walled carbon nanotube prepared by the preparation method described in the above technical solution; forming the mixed slurry into a film to obtain a wet film; and heating and curing the wet film to obtain the n-type doped single-walled carbon nanotube thermoelectric film. The preparation method provided by the present invention is to mix the n-type doped single-walled carbon nanotube and the organic adhesive in an organic solvent, and since PVP is coated on the surface of SWCNTs, the dispersibility between the n-type doped single-walled carbon nanotubes and between the n-type doped single-walled carbon nanotube and the organic adhesive is effectively improved, and the thermoelectric film obtained by curing the film has good flexibility and uniformity, and the preparation method provided by the present invention is simple, low-cost, easy to implement, and is expected to be applied on a large scale.
[0026] The present invention provides an n-type doped single-walled carbon nanotube thermoelectric film prepared by the preparation method described in the above technical solution, wherein the n-type doped single-walled carbon nanotube thermoelectric film is a self-supporting flexible film. The n-type doped single-walled carbon nanotube thermoelectric film provided by the present invention is a self-supporting flexible film, and has good flexibility and uniformity, and is expected to be prepared with the existing p-type thermoelectric film into a flexible thermoelectric device that can be worn by the human body. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a Raman spectrum of the n-type doped SWCNTs film prepared in Example 1 of the present invention;
[0028] Figure 2 is a partial enlarged view of the Raman spectrum of the n-type doped SWCNTs film prepared in Example 1 of the present invention;
[0029] Figure 3 is a scanning electron microscope image of the n-type doped SWCNTs film prepared in Example 2 of the present invention;
[0030] Figure 4 is the Seebeck coefficient diagram of the n-type doped SWCNTs films prepared in Examples 1, 2, and 3 of the present invention;
[0031] Figure 5 Graphs showing the conductivity and power factor of n-type doped SWCNTs films prepared in Examples 1, 2, and 3 of the present invention. DETAILED DESCRIPTION
[0032] The invention provides an n-type doped single-wall carbon nanotube, comprising a single-wall carbon nanotube modified by covalent grafting of polyvinyl pyrrolidone.
[0033] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0034] In the present invention, the mass ratio of the polyvinyl pyrrolidone to the single-walled carbon nanotubes is (2-4):1, and is preferably 2:1, 3:1 or 4:1.
[0035] The present invention provides a method for preparing n-type doped single-walled carbon nanotubes as described in the above technical solution, comprising the following steps:
[0036] Mixing polyvinyl pyrrolidone, single-walled carbon nanotubes and an alcohol solvent to obtain a suspension;
[0037] In a protective gas atmosphere, the suspension is heated to perform a grafting reaction to obtain the n-type doped single-walled carbon nanotubes.
[0038] The present invention mixes polyvinyl pyrrolidone, single-walled carbon nanotubes and an alcohol solvent (hereinafter referred to as the first mixture) to obtain a suspension.
[0039] In the present invention, the alcohol solvent is preferably ethylene glycol.
[0040] In the present invention, the mass ratio of the polyvinyl pyrrolidone to the single-walled carbon nanotubes is (2-4):1, and is preferably 2:1, 3:1 or 4:1.
[0041] The present invention has no special requirement on the amount of ethylene glycol used, as long as it can ensure the grafting reaction.
[0042] In the present invention, the first mixing is preferably performed under stirring conditions, and the stirring speed is preferably 1100 rad / min.
[0043] After obtaining the suspension, the present invention heats the suspension in a protective gas atmosphere to perform a grafting reaction to obtain the n-type doped single-walled carbon nanotubes.
[0044] In the present invention, the protective gas atmosphere is preferably an inert gas atmosphere.
[0045] In the present invention, the temperature of the grafting reaction is preferably 270 to 280°C, more preferably 275°C.
[0046] In the present invention, the holding time of the grafting reaction is preferably 15 to 24 hours, more preferably 20 hours.
[0047] In the present invention, the grafting reaction is preferably carried out under stirring, and the stirring speed is preferably 1100 rad / min. In a specific embodiment of the present invention, the stirring is preferably magnetic stirring.
[0048] In the present invention, the grafting reaction is preferably carried out in a reactor with a magnetic heating stirrer.
[0049] In the present invention, the grafting reaction directly obtains a grafting reaction liquid. After the grafting reaction, the present invention preferably further comprises sequentially subjecting the grafting reaction liquid to alcohol precipitation, solid-liquid separation and washing to obtain the n-type doped single-walled carbon nanotubes; the alcohol solvent used for the alcohol precipitation is isopropanol.
[0050] In the present invention, the alcohol precipitation is preferably performed by mixing the grafting reaction solution with an alcohol solvent for alcohol precipitation. In the present invention, the volume ratio of the alcohol solvent for alcohol precipitation to the grafting reaction solution is preferably 1:1.
[0051] The present invention preferably performs solid-liquid separation on the alcohol precipitation reaction liquid obtained by the alcohol precipitation. In the present invention, the solid-liquid separation is preferably centrifugal. The present invention has no special requirements on the specific implementation process of the ion.
[0052] The present invention preferably washes the solid product obtained by the solid-liquid separation, and in the present invention, the washing solvent is preferably ethanol, and in the present invention, the number of washings is preferably 3. The present invention preferably removes unreacted raw materials and ethylene glycol by washing.
[0053] The present invention provides the use of the n-type doped single-walled carbon nanotubes described in the above technical solution or the n-type doped single-walled carbon nanotubes prepared by the preparation method described in the above technical solution as thermoelectric materials.
[0054] The present invention provides a method for preparing an n-type doped single-walled carbon nanotube thermoelectric film, comprising the following steps:
[0055] The n-type doped single-walled carbon nanotubes, an organic binder and an organic solvent are mixed to obtain a mixed slurry; the n-type doped single-walled carbon nanotubes are the n-type doped single-walled carbon nanotubes described in the above technical solution or the n-type doped single-walled carbon nanotubes prepared by the preparation method described in the above technical solution;
[0056] Forming the mixed slurry into a film to obtain a wet film;
[0057] The wet film is heated and cured to obtain the n-type doped single-walled carbon nanotube thermoelectric film.
[0058] The present invention mixes the n-type doped single-walled carbon nanotubes, an organic adhesive and an organic solvent (hereinafter referred to as the second mixture) to obtain a mixed slurry; the n-type doped single-walled carbon nanotubes are the n-type doped single-walled carbon nanotubes described in the above technical solution or the n-type doped single-walled carbon nanotubes prepared by the preparation method described in the above technical solution.
[0059] In the present invention, the organic binder preferably includes polyvinylidene fluoride.
[0060] In the present invention, the organic solvent is preferably N,N-dimethylformamide (DMF).
[0061] In the present invention, the mass ratio of the n-type doped single-walled carbon nanotubes to the organic binder is preferably (4-6):1, more preferably 5:1.
[0062] The present invention has no special requirement on the amount of the organic solvent, as long as it can ensure that the n-type doped single-walled carbon nanotubes and the organic adhesive are mixed evenly.
[0063] In the present invention, the second mixing is preferably carried out under ultrasonic conditions, the power of the ultrasound is preferably 360 W; the frequency of the ultrasound is preferably 40 Hz, and the time of the ultrasound is preferably 1 h.
[0064] After obtaining the mixed slurry, the present invention forms a film from the mixed slurry to obtain a wet film.
[0065] In the present invention, the film forming is preferably performed by coating the mixed slurry on a substrate surface to form a film.
[0066] In the present invention, the material of the substrate is preferably glass.
[0067] In the present invention, the coating is preferably spin coating.
[0068] In the present invention, the thickness of the wet film is preferably ∼60 μm.
[0069] After obtaining the wet film, the present invention heats and solidifies the wet film to obtain the n-type doped single-walled carbon nanotube thermoelectric film.
[0070] In the present invention, the curing temperature is preferably 75-80°C, more preferably 80°C.
[0071] In the present invention, the curing heat preservation time is preferably 1 to 3 hours, more preferably 3 hours.
[0072] In the present invention, the film formation is preferably performed on the surface of a substrate, and after the curing, the present invention preferably peels the n-type doped single-walled carbon nanotube thermoelectric film from the substrate.
[0073] The present invention has no special requirements on the specific implementation process of the stripping.
[0074] In the present invention, the thickness of the n-type doped single-walled carbon nanotube thermoelectric film is preferably ˜30 μm.
[0075] The present invention provides an n-type doped single-walled carbon nanotube thermoelectric film prepared by the preparation method described in the above technical solution, wherein the n-type doped single-walled carbon nanotube thermoelectric film is a self-supporting flexible film.
[0076] The n-type doped single-walled carbon nanotube thermoelectric film provided by the present invention has uniform morphology, independent self-supporting performance, and good flexibility and uniformity. It is expected to be prepared with the existing p-type thermoelectric film into a flexible thermoelectric device that can be worn by the human body.
[0077] In order to further illustrate the present invention, the technical solution provided by the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0078] Example 1
[0079] Weigh 0.098232 g of PVP and 0.032744 g of SWCNTs and mix with ethylene glycol to obtain a suspension;
[0080] Under an inert gas atmosphere, the suspension was transferred to a reaction kettle and placed in a magnetic heating stirrer, heated and stirred at a stirring speed of 1100 rad / min, and reacted at 275°C for 20 hours to obtain a grafting reaction liquid;
[0081] After the grafting reaction liquid was cooled to room temperature, it was precipitated with isopropanol in a volume ratio of 1:1 to the grafting reaction liquid, and then centrifuged to obtain a solid product. The solid product was washed three times with ethanol to remove unreacted raw materials and ethylene glycol to obtain n-type doped single-walled carbon nanotubes.
[0082] n-type doped single-walled carbon nanotubes and 0.0109 g PVDF were mixed in DMF at a mass ratio of 5:1 and subjected to ultrasonic treatment for 1 h, with an ultrasonic power of 360 W and an ultrasonic frequency of 40 Hz to obtain a mixed slurry;
[0083] The mixed slurry was coated on glass to obtain a wet film with a thickness of ∼60 μm;
[0084] The wet film was cured at 80°C for 3 hours and then peeled off from the glass to obtain an independently supportable n-type doped single-walled carbon nanotube thermoelectric film with a thickness of ∼30 μm.
[0085] The structure and morphology of n-type doped single-walled carbon nanotube thermoelectric films were analyzed by Raman spectroscopy. The characteristic Raman peaks of SWCNTs include D peak (~1341cm -1 ) and G peak (~1592cm -1 ), respectively related to defect-induced resonant scattering and sp 2 It is related to the in-plane stretching vibration of hybridized carbon atoms. Figures 1-2 The Raman spectrum shows that the n-type doped single-walled carbon nanotube thermoelectric film prepared in this example is SWCNTs, and the spectrum shows that the G diffraction peak of the SWCNTs film (n-type doped single-walled carbon nanotube thermoelectric film) after covalent grafting with PVP is blue-shifted compared with the original carbon tube, from 1592.48 cm -1 To 1591.11cm -1 , which indicates that PVP and CNTs SP 2 Hybridization bonding occurs, and electrons are transferred from PVP to SWCNTs, which is consistent with the n-type Seebeck coefficient measured by PTM.
[0086] Example 2
[0087] Weigh 0.130976 g of PVP and 0.032744 g of SWCNTs and mix with ethylene glycol to obtain a suspension;
[0088] Under an inert gas atmosphere, the suspension was transferred to a reaction kettle and placed in a magnetic heating stirrer, heated and stirred at a stirring speed of 1100 rad / min, and reacted at 275°C for 20 hours to obtain a grafting reaction liquid;
[0089] After the grafting reaction liquid was cooled to room temperature, it was precipitated with isopropanol in a volume ratio of 1:1 to the grafting reaction liquid, and then centrifuged to obtain a solid product. The solid product was washed three times with ethanol to remove unreacted raw materials and ethylene glycol to obtain n-type doped single-walled carbon nanotubes.
[0090] n-type doped single-walled carbon nanotubes and 0.0109 g PVDF were mixed in DMF at a mass ratio of 5:1 and subjected to ultrasonic treatment for 1 h, with an ultrasonic power of 360 W and an ultrasonic frequency of 40 Hz to obtain a mixed slurry;
[0091] The mixed slurry was coated on glass to obtain a wet film with a thickness of ∼60 μm;
[0092] The wet film was cured at 80°C for 3 hours and then peeled off from the glass to obtain an independently supportable n-type doped single-walled carbon nanotube thermoelectric film with a thickness of ∼30 μm.
[0093] The surface morphology of the n-type doped single-walled carbon nanotube thermoelectric film sample prepared in this embodiment was observed by scanning electron microscopy. The SWCNTs in the n-type doped single-walled carbon nanotube thermoelectric film prepared in this embodiment were well dispersed and the film surface was uniform. Figure 3 As shown. Compared with SWCNTs without PVP, SWCNTs with PVP added are distinct and evenly dispersed. This is mainly because PVP adsorbed on carbon tubes can act as a surfactant and dispersant, reducing the agglomeration of carbon tubes and playing a role in fully and evenly dispersing carbon tubes. In addition, the preparation process is heated and stirred at the same time, so that PVP can fully coat SWCNTs, which is beneficial to reduce the agglomeration between carbon tubes.
[0094] Example 3
[0095] Weigh 0.065488 g of PVP and 0.032744 g of SWCNTs and mix with the ethylene glycol solution to obtain a suspension;
[0096] Under an inert gas atmosphere, the suspension was transferred to a reaction kettle and placed in a magnetic heating stirrer, heated and stirred at a stirring speed of 1100 rad / min, and reacted at 275°C for 20 hours to obtain a grafting reaction liquid;
[0097] After the grafting reaction liquid was cooled to room temperature, it was precipitated with isopropanol in a volume ratio of 1:1 to the grafting reaction liquid, and then centrifuged to obtain a solid product. The solid product was washed three times with ethanol to remove unreacted raw materials and ethylene glycol to obtain n-type doped single-walled carbon nanotubes.
[0098] n-type doped single-walled carbon nanotubes and 0.0109 g PVDF were mixed in DMF at a mass ratio of 5:1 and subjected to ultrasonic treatment for 1 h, with an ultrasonic power of 360 W and an ultrasonic frequency of 40 Hz to obtain a mixed slurry;
[0099] The mixed slurry was coated on glass to obtain a wet film with a thickness of ∼60 μm;
[0100] The wet film was cured at 80°C for 3 hours and then peeled off from the glass to obtain an independently supportable n-type doped single-walled carbon nanotube thermoelectric film with a thickness of ∼30 μm.
[0101] The room temperature thermoelectric characteristic evaluation device PTM was used to test the Seebeck coefficient of the n-type doped single-walled carbon nanotube thermoelectric film samples prepared in Examples 1 to 3 as a function of PVP content. Figure 4 As shown. The Seebeck coefficients of the n-type doped single-walled carbon nanotube thermoelectric films prepared in the embodiments of the present invention are all negative numbers, indicating that the prepared n-type doped single-walled carbon nanotube thermoelectric films are all n-type semiconductors. Moreover, as the PVP content increases, the Seebeck coefficient of the SWCNTs film increases. The n-type doped single-walled carbon nanotube thermoelectric film prepared when the mass ratio PVP:SWCNTs=4:1 has the largest Seebeck coefficient, which is -53μV·K -1 , indicating that the covalent bond interaction between PVP and SWCNTs can be further strengthened by the solvothermal method, and PVP provides electrons to SWCNTs, making the SWCNTs film exhibit n-type conductive behavior.
[0102] The room temperature thermoelectric characteristic evaluation device PTM was used to test the conductivity of the n-type doped single-walled carbon nanotube thermoelectric film samples prepared in Examples 1 to 3 as a function of PVP content, and the power factor as a function of PVP content was obtained. Figure 5 By comparison, it is found that the conductivity of the n-type doped single-walled carbon nanotube thermoelectric films prepared in Examples 1 to 3 decreases with the increase of PVP content, which is opposite to the change trend of the Seebeck coefficient. Power factor PF = S 2 σ, where S refers to the Seebeck coefficient and σ refers to the electrical conductivity of the material. Therefore, the n-type doped single-walled carbon nanotube thermoelectric film prepared with a final mass ratio of PVP:SWCNTs = 3:1 showed an optimal power factor of -72.59μW·m -1 ·K -2 .
[0103] In summary, compared with traditional inorganic thermoelectric materials, the n-type doped single-walled carbon nanotube thermoelectric film provided by the present invention has not only a higher Seebeck coefficient, electrical conductivity and power factor, but also good flexibility and mechanical strength performance, and is expected to be combined with existing high-performance p-type thermoelectric film materials and applied to flexible wearable thermoelectric devices. And compared with other methods for preparing thermoelectric film materials, the method for preparing the n-type doped single-walled carbon nanotube thermoelectric film provided by the present invention is simple, low-cost, easy to implement, and is expected to be applied on a large scale.
[0104] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing n-type doped single-walled carbon nanotubes, characterized in that: The following steps are involved: Mixing polyvinyl pyrrolidone, single-walled carbon nanotubes and ethylene glycol to obtain a suspension; the mass ratio of the polyvinyl pyrrolidone to the single-walled carbon nanotubes is (2-4):1; In a protective gas atmosphere, heating the suspension to carry out a grafting reaction to obtain the n-type doped single-walled carbon nanotubes; the grafting reaction temperature is 270-280° C., and the grafting reaction insulation time is 15-24 h; The n-type doped single-walled carbon nanotubes include single-walled carbon nanotubes modified by covalent grafting of polyvinyl pyrrolidone.
2. The preparation method according to claim 1, characterized in that: The grafting reaction directly obtains a grafting reaction liquid. After the grafting reaction, the grafting reaction liquid is sequentially subjected to alcohol precipitation, solid-liquid separation and washing to obtain the n-type doped single-walled carbon nanotubes. The alcohol solvent used for the alcohol precipitation is isopropanol.
3. A method for preparing an n-type doped single-walled carbon nanotube thermoelectric film, characterized in that: The following steps are involved: The n-type doped single-walled carbon nanotubes, an organic binder and an organic solvent are mixed to obtain a mixed slurry; the n-type doped single-walled carbon nanotubes are n-type doped single-walled carbon nanotubes prepared by the preparation method according to claim 1 or 2; Forming the mixed slurry into a film to obtain a wet film; heating and curing the wet film to obtain the n-type doped single-walled carbon nanotube thermoelectric film; The n-type doped single-walled carbon nanotube thermoelectric film is a self-supporting flexible film.
4. The preparation method according to claim 3, characterized in that: The organic adhesive includes polyvinylidene fluoride, and the mass ratio of the n-type doped single-walled carbon nanotube to the organic adhesive is (4-6):
1.