A high-performance nuclear waste solidification material and preparation method thereof
By using low-thermal silicate cement and barium silicate cement composite, metakaolin, zeolite powder, activated carbon/silane black and barite aggregate and other materials, the stability of cement-based materials in curing and The problem of insufficient shielding effect has achieved high-performance nuclear waste solidification materials, meeting the curing and engineering application requirements of the nuclear industry.
Patent Information
- Application Number
- CN202211644939.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-16
AI Technical Summary
When curing low-radioactive solid wastes, existing cement-based materials have problems such as mud water leakage, isolation, loss of fluidity, insufficient fixed body strength, poor anti-chlorine ion permeability and unstable volume, and it is difficult to meet the engineering scale tolerance of the nuclear industry. sexual requirements and shielding effect requirements.
Low-thermal silicate cement and barium silicate cement are used as cementitious materials, combined with metakaolin, zeolite powder and activated carbon/salin black as mineral blends, barite aggregate and quartz sand as fine aggregates, and Add water reducing agent, defoaming agent and thickening agent to form a high-performance cement-based nuclear waste solidification material to improve the workingability, flowability, strength, durability and shielding effect of the solidification material.
It realizes the stable workingability, large flow, high strength, good durability, wide fault tolerance range, and high nuclide adsorption shielding of the curing material, meets the curing standards and engineering application requirements of the nuclear industry, reduces radioactive hazards, and improves the Shielding effect and transport efficiency of waste packs.
Smart Images

Figure BDA0004002321500000131 
Figure BDA0004002321500000141
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nuclear waste solidification, and in particular relates to a high-performance cement-based nuclear waste solidification material and a preparation method thereof. Background Art
[0002] With the development of the nuclear industry, radioactive waste is produced in large quantities. How to safely, safely and efficiently handle and dispose of these wastes is an important issue that nuclear power plants and reprocessing plants must face.
[0003] Medium and low-level radioactive solid waste (hereinafter referred to as medium and low-level solid waste) exists in large quantities both in operating nuclear power plants and in the field of nuclear facility decommissioning. Using cement-based materials to fix them is an effective method. The National Nuclear Industry Standard EJ1186-2005 "Identification of the Characteristics of Radioactive Waste Bodies and Waste Packages" has set clear requirements for the indicators of cement mortar used for fixing the above solid waste.
[0004] However, there are many types of low- and intermediate-level radioactive solid wastes with varied compositions. Some of them contain substances that are easy to rust, have low density, large volume fluctuations, and poor compatibility with cement. When these wastes are solidified using conventional cement-based materials, problems such as mud seepage, segregation, uncontrolled fluidity, insufficient strength of the fixed body after hardening, poor resistance to chloride ion permeability, and even unstable volume may occur.
[0005] On the other hand, whether cement fixation meets the standard requirements and disposal requirements, its formula must take into account the fault tolerance of the engineering scale, because the measurement deviation and systematic error in the engineering field are essentially unable to achieve the accuracy of small-scale laboratory tests, which puts higher requirements on the formula envelope.
[0006] In addition, after the waste bag is fixed with cement, it must meet the shielding requirements before it can be transported. Conventional cement fixing formulas often focus on the physical properties of the fixing material, and there is a lack of research on how to further improve the shielding effect of the waste bag.
[0007] In view of this, it is necessary to develop a nuclear waste solidification material that can meet the solidification standard requirements and actual engineering application requirements and maximize the shielding effect of the waste package. Summary of the invention
[0008] The present invention solves the above problems through raw material optimization, ratio selection test and engineering verification research, and proposes a high-performance cement-based nuclear waste solidification material.
[0009] The purpose of the present invention is to solve various fixing problems generated in the process of nuclear industry application, so as to achieve the adsorption and shielding of solid waste with radioactive contamination, thereby reducing the radioactive hazards of solid nuclear waste, improving the efficiency of waste package transportation, and achieving the purpose of convenient storage, management, transportation, etc. Compared with the prior art, the material of the present invention has the advantages of stable workability, high fluidity, high strength, good durability, wide fault tolerance range, high nuclide adsorption and shielding, and stable performance.
[0010] The present invention provides a nuclear waste solidifying material for solidifying solid waste with radioactive contamination (preferably solid waste with low or medium radioactive levels), comprising the following components in parts by weight: 40-50 parts of cementitious material; 20-60 parts of fine aggregate; 6-12 parts of mineral admixture; and 0.5-2.0 parts of admixture; wherein the cementitious material comprises low-heat silicate cement and barium silicate cement, the fine aggregate comprises barite aggregate and quartz sand, the mineral admixture comprises metakaolin, zeolite powder and a first material, and the first material is at least one of activated carbon and white carbon black.
[0011] Among them, 40-50 parts of cementitious materials contain: 30-35 parts of low-heat silicate cement and 10-15 parts of barium silicate cement.
[0012] Among them, 6-12 parts of mineral admixtures contain: 4-6 parts of metakaolin, 1-3 parts of zeolite powder; and 1-3 parts of the first material.
[0013] Among them, 20-60 parts of fine aggregate contain 10-50 parts of barite aggregate and 50-10 parts of quartz sand.
[0014] Wherein, the mesh size of the fine aggregate is 10-70.
[0015] Among them, 0.5-2.0 parts of admixtures contain: 0.3-1.0 parts of water reducing agent; 0.1-0.3 parts of defoaming agent; 0.1-0.3 parts of thickener.
[0016] Among them, the water reducer is preferably a polycarboxylate water reducer; the defoamer is preferably a solid particle defoamer; the thickener is preferably a cellulose ether; the cellulose ether is preferably hydroxypropyl cellulose ether or methyl cellulose ether, more preferably hydroxypropyl methyl cellulose ether with a viscosity of 20000-100000.
[0017] The present invention also provides a method for preparing the nuclear waste solidified material, comprising: mixing the components of the nuclear waste solidified material in proportion to obtain the nuclear waste solidified material.
[0018] The present invention also provides a method for solidifying low- and medium-level radioactive solid wastes using the above-mentioned nuclear waste solidification material, comprising the following steps:
[0019] Adding water to the nuclear waste solidified material at a weight ratio of 0.11 to 0.17 of water to material ratio, and mixing well to obtain a nuclear waste solidified material mixture;
[0020] The nuclear waste solidification material mixture is evenly mixed with the low and medium radioactive level solid wastes that need to be treated, and poured, stored and disposed of according to the on-site construction requirements.
[0021] The present invention has the following beneficial technical effects:
[0022] (1) In terms of cementitious materials, the present invention uses a compound of low-heat silicate cement and barium silicate cement. The medium- and low-radioactive cement fixed bodies prepared using traditional ordinary silicate cement often have the problems of high heat release rate during hardening and cracking of the fixed body after hardening. In general, the above problems can be avoided by corresponding manual intervention methods (such as heat preservation after pouring, regular watering, covering with plastic film for maintenance, etc.). However, for radioactive environments, these operations are not conducive to the health of personnel. At the same time, such operations will also produce more secondary waste, increasing the difficulty and cost of treatment. Therefore, how to ensure that the cement fixed body maintains a low temperature rise and heat release rate during hardening plays an important role in increasing the volume stability of the cement fixed body. On the other hand, the most important task of the cement fixed body is to achieve the sealed packaging of radioactive waste. If the volume stability of the cement fixed body itself changes, the function of the sealed packaging will also fail. Therefore, it is very important to select a cementitious material with low hydration heat and high durability for nuclear waste solidification / fixation. The present invention uses a compound of low-heat silicate cement and barium silicate cement as a cementitious material. Compared with other cements, low-heat silicate cement can significantly reduce the hydration heat release rate, which is beneficial to reduce the heat release rate of early cement, reduce thermal deformation during hardening, improve the volume stability and durability of the matrix, make the structure more stable, and have higher density, which is more conducive to regulating the early strength of the material. At the same time, barium silicate cement is compounded and used. Barium silicate cement has a strong absorption and shielding effect on radiation, which can improve the shielding ability of the fixed body to radiation, effectively improve the shielding effect of the waste bag, and reduce the radioactivity level.
[0023] (2) In terms of mineral admixtures, the present invention uses a compound of metakaolin, zeolite powder, and at least one selected from activated carbon and white carbon black. + ) environment is commonly found in the nuclear waste reprocessing stage, and metakaolin can effectively adsorb Na + , improve the anti-efflorescence ability of the fixed body, reduce the risk of poor surface density caused by efflorescence, and further improve the stability of the fixed body. This feature is effective for some nuclides (such as 137 Cs) with Na in the system +It plays an important role in the free precipitation and deposition on the surface of the structure. Zeolite can directly adsorb some nuclides that are difficult to be solidified / co-precipitated by cement. The adsorption effect of zeolite and the compacting effect of low-heat silicate cement are superimposed to further inhibit the diffusion of nuclides. The co-addition of kaolin and zeolite powder will exert a superimposed effect and more effectively improve the fixation effect of the system. Activated carbon and / or white carbon black can further improve the adsorption capacity of molecular radioactive waste that may exist in the waste, and at the same time cooperate with other components to improve the stability and water retention of the fixed body mud, and further consolidate the fixation effect of the fixed body. The organic compound of the above materials can synergistically adsorb and retain nuclides ions and nuclide molecules, while increasing the density of the fixed body, improving the resistance of the fixed body to chloride ion permeability and corrosion resistance, which is beneficial to improving the adsorption and density of the material to nuclides.
[0024] (3) In terms of fine aggregate, the present invention uses a combination of barite aggregate and quartz sand aggregate. The combination of barite aggregate can improve the radiation shielding effect, thereby further reducing the surface dose rate of the waste bag. The synergistic effect of the barite aggregate and quartz sand can ensure that the solidified material has a higher adsorption and isolation effect on radiation, and at the same time, the solidified material can have higher mechanical properties and density.
[0025] (4) In terms of admixtures, the present invention uses water reducers, thickeners, defoamers, etc. to improve the fluidity, stability, fault tolerance and physical and mechanical properties of the fixed body. Specifically, the admixture is preferably a polycarboxylic acid water reducer, and the water reduction rate of the polycarboxylic acid water reducer is ≥25%. The use of a water reducer with a water reduction rate of ≥25% can greatly reduce the water consumption of the material, so that the material has good fluidity and strength. The defoamer is preferably a solid particle type defoamer, which has a strong defoaming ability and can make the material have good density without affecting the basic performance of the system. The thickener is preferably a cellulose ether, more preferably hydroxypropyl cellulose ether or methyl cellulose ether, more preferably hydroxypropyl methyl cellulose ether with a viscosity of 20000-100000, and its surface activity ensures that the gelling material is effectively and evenly distributed in the system, making the mortar system more stable, adjusting the viscosity and fluidity of the material, and giving the material water retention and density.
[0026] (5) In the prior art, barium silicate cement and barite are often used in the field of radiation-proof concrete, and there is almost no precedent for their use in the field of fixing medium- and low-level solid waste; activated carbon and white carbon black are often used in industries such as water treatment or coatings, and there is almost no precedent for their use in the field of formulating and developing medium- and low-level solid waste; although there are precedents for the application of metakaolin and zeolite powder in this field, there is almost no precedent for their use in terms of scientific compatibility of the above materials to achieve a more ideal effect. The present invention uses low-heat silicate cement and barium silicate cement as a cementitious material, metakaolin, zeolite powder and at least one selected from white carbon black and activated carbon as a mineral admixture, and barite aggregate and quartz sand as a fine aggregate. The above cementitious material, mineral admixture and fine aggregate work synergistically, so that the obtained nuclear waste solidification material has the advantages of stable workability, high fluidity, high strength, controllable strength, good workability, outstanding shielding effect and good durability.
[0027] (7) The nuclear waste solidification material of the present invention is tested in accordance with EJ1186-2005 "Identification of Characteristics of Radioactive Waste Bodies and Waste Packages", GB12711-2018 "Safety Standards for Low and Medium Level Radioactive Solid Waste Packages", GB8076-2008 "Concrete Admixtures", GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures", and JGJ / T192-2009 "Technical Specifications for Application of Rebar Rust Inhibitors", wherein the fluidity of the nuclear waste solidification material is between 310 and 370 mm, the 28-day compressive strength is between 90 MPa and 130 MPa, the 90-day compressive strength is between 110 MPa and 140 MPa, the 28-day chloride ion permeability is less than 1000C, the surface dose rate reduction effect is more than 90%, the mud has no water exudation and segregation when the water consumption fluctuates within the system error, and the fluidity is greater than 310 mm, and the corrosion resistance is outstanding. The above performance not only meets the requirements of EJ1186-2005 "Characterization of Radioactive Waste Bodies and Waste Packages", but also can adapt to the fault tolerance of the engineering scale and the stability under error conditions. DETAILED DESCRIPTION
[0028] The present invention will be described in further detail below in conjunction with specific embodiments. However, it should be understood that these embodiments are only for illustration and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims of the present application.
[0029] Example 1
[0030] This embodiment provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0031] 35 parts of low-heat silicate cement (P·LH42.5); 15 parts of barium silicate cement; 5 parts of metakaolin; 2 parts of zeolite powder; 2 parts of activated carbon; 1 part of polycarboxylic acid water reducer (water reduction rate ≥25%); 0.1 part of defoamer; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 20 parts of barite aggregate; 20 parts of quartz sand.
[0032] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0033] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0034] The nuclear waste solidified material prepared above was fully mixed with 14 parts by weight of water at a speed of 200 r / min for 3 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~17 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0035] Example 2
[0036] This embodiment provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0037] 35 parts of low-heat silicate cement; 15 parts of barium silicate cement; 5 parts of metakaolin; 2 parts of zeolite powder; 2 parts of activated carbon; 1 part of polycarboxylic acid water reducer (water reduction rate ≥ 25%); 0.1 part of defoamer; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 20 parts of barite aggregate; 20 parts of quartz sand.
[0038] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0039] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0040] The nuclear waste solidified material prepared above was fully mixed with 11 parts by weight of water at a speed of 200 r / min for 3 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~19 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0041] Example 3
[0042] This embodiment provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0043] 35 parts of low-heat silicate cement; 15 parts of barium silicate cement; 5 parts of metakaolin; 2 parts of zeolite powder; 2 parts of activated carbon; 1 part of polycarboxylic acid water reducer (water reduction rate ≥ 25%); 0.1 part of defoamer; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 20 parts of barite aggregate; 20 parts of quartz sand.
[0044] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0045] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0046] The nuclear waste solidified material prepared above was fully mixed with 17 parts by weight of water at a speed of 200 r / min for 5 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~16 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0047] Example 4
[0048] This embodiment provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0049] 35 parts of low-heat silicate cement; 15 parts of barium silicate cement; 5 parts of metakaolin; 2 parts of zeolite powder; 2 parts of white carbon black; 1 part of polycarboxylic acid water reducer (water reduction rate ≥ 25%); 0.1 part of defoamer; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 20 parts of barite aggregate; 20 parts of quartz sand.
[0050] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0051] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0052] The nuclear waste solidified material prepared above was fully mixed with 14 parts by weight of water at a speed of 200 r / min for 3 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~15 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0053] Comparative Example 1
[0054] This comparative example provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0055] 35 parts of low-heat silicate cement; 15 parts of barium silicate cement; 5 parts of metakaolin; 2 parts of zeolite powder; 2 parts of activated carbon; 1 part of polycarboxylic acid water reducer (water reduction rate ≥ 25%); 0.1 part of defoaming agent; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 40 parts of quartz sand.
[0056] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0057] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0058] The nuclear waste solidified material prepared above was fully mixed with 14 parts by weight of water at a speed of 200 r / min for 3 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~16 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0059] Comparative Example 2
[0060] This comparative example provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0061] 35 parts of low-heat Portland cement; 15 parts of ordinary Portland cement; 5 parts of metakaolin; 2 parts of zeolite powder; 2 parts of activated carbon; 1 part of polycarboxylic acid water reducer (water reduction rate ≥ 25%); 0.1 part of defoamer; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 20 parts of barite aggregate; 20 parts of quartz sand.
[0062] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0063] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0064] The nuclear waste solidified material prepared above was fully mixed with 14 parts by weight of water at a speed of 200 r / min for 3 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~17 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0065] Comparative Example 3
[0066] This comparative example provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0067] 50 parts of ordinary Portland cement; 5 parts of metakaolin; 2 parts of zeolite powder; 2 parts of activated carbon; 1 part of polycarboxylic acid water reducer (water reduction rate ≥ 25%); 0.1 part of defoamer; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 20 parts of barite aggregate; 20 parts of quartz sand.
[0068] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0069] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0070] The nuclear waste solidified material prepared above was fully mixed with 14 parts by weight of water at a speed of 200 r / min for 3 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~16 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0071] Comparative Example 4
[0072] This comparative example provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0073] 35 parts of low-heat silicate cement; 15 parts of barium silicate cement; 5 parts of metakaolin; 2 parts of activated carbon; 1 part of polycarboxylic acid water reducer (water reduction rate ≥ 25%); 0.1 part of defoamer; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 20 parts of barite aggregate; 20 parts of quartz sand.
[0074] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0075] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0076] The nuclear waste solidified material prepared above was fully mixed with 14 parts by weight of water at a speed of 200 r / min for 3 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~17 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0077] Comparative Example 5
[0078] This comparative example provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0079] 35 parts of low-heat silicate cement; 15 parts of barium silicate cement; 2 parts of zeolite powder; 2 parts of activated carbon; 1 part of polycarboxylic acid water reducer (water reduction rate ≥ 25%); 0.1 part of defoamer; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 20 parts of barite aggregate; 20 parts of quartz sand.
[0080] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0081] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0082] The nuclear waste solidified material prepared above was fully mixed with 14 parts by weight of water at a speed of 200 r / min for 3 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~18 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0083] Comparative Example 6
[0084] This comparative example provides a nuclear waste solidification material, which comprises the following components in parts by weight according to the component formula shown in Table 1:
[0085] 35 parts of low-heat silicate cement; 15 parts of barium silicate cement; 5 parts of metakaolin; 2 parts of zeolite powder; 1 part of polycarboxylic acid water reducer (water reduction rate ≥ 25%); 0.1 part of defoamer; 0.1 part of hydroxypropyl methylcellulose ether (viscosity: 100000); 20 parts of barite aggregate; 20 parts of quartz sand.
[0086] The preparation method of the nuclear waste solidified material comprises the following steps: weighing each component by weight and mixing them evenly to obtain the nuclear waste solidified material.
[0087] The method for using the above-mentioned nuclear waste solidification material comprises the following steps:
[0088] The nuclear waste solidified material prepared above was fully mixed with 14 parts by weight of water at a speed of 200 r / min for 3 minutes, and the required medium and low-level metal nuclear waste (surface dose rate ~17 mSv / h) was poured, and performance sampling test was carried out simultaneously.
[0089] For the fixed body prepared from the nuclear waste solidification material described in each embodiment and comparative example, the initial fluidity, 7-day compressive strength, 28-day compressive strength, 90-day compressive strength, and 28d chloride ion permeability (electric flux) were tested according to EJ1186-2005. The fixed body was tested for water seepage and segregation with reference to GB / T50080-2016, and it was found that there was no corrosion to the steel bars with reference to GB8076-2008 and JGJ / T192-2009. The surface dose rate reduction effect was tested according to GB12711-2018. The test results are shown in Table 2.
[0090]
[0091]
[0092] The above-mentioned Examples 1-3 illustrate the reliability and practicality of the nuclear waste solidified material formula of the present invention under the condition of water consumption fluctuation. Because in actual application, the weight of the solidified material can be accurately controlled when leaving the factory, and the metering of the mixing water is affected by the equipment system error and metering error, and it is often impossible to accurately control it, but the water consumption will obviously affect the overall performance of the cement body. Therefore, if the solidified material formula is not good, the fluctuation of water consumption will greatly affect the performance of the final solidified body. However, in the case of water consumption fluctuation (11-17 parts by weight fluctuation) of Examples 1-3 of the present invention, a solidified body with good performance can still be obtained. In particular, Example 3, its water consumption is as high as 17 parts by weight, and the results show that even if the water consumption of Example 3 is greatly increased, the surface dose rate reduction effect of Example 3 is not lower than that of other comparative examples with lower water consumption, and even has a certain degree of improvement. These results all confirm the reliability and practicality of the nuclear waste solidified material formula of the present invention.
[0093] By comparing Example 1 with Comparative Example 1, it can be found that when the barite aggregate is replaced by quartz sand aggregate, that is, when only quartz sand is used in the fine aggregate instead of barite aggregate and quartz sand, the surface dose rate reduction effect is significantly reduced, which shows that barite plays a positive correlation role in reducing radiation.
[0094] By comparing Example 1 with Comparative Example 2, it can be found that when barium silicate cement is replaced by ordinary silicate cement, the surface dose rate reduction effect is significantly reduced, which means that barium silicate cement plays a positive role in reducing radiation.
[0095] By comparing Example 1 with Comparative Example 3, it can be found that when only ordinary Portland cement is used as the cementitious material, the surface dose rate reduction effect decreases and the resistance to chloride ion permeability becomes worse, which can be explained that low-heat Portland cement plays a positive correlation role in reducing radionuclide radiation and improving the density of the fixed body.
[0096] By comparing Example 1 with Comparative Examples 4 and 5, it can be found that when the system does not contain zeolite, the surface dose rate reduction effect shows a downward trend; when the system does not contain metakaolin, the resistance to chloride ion permeability deteriorates and the surface dose rate reduction effect shows a downward trend. This shows that metakaolin and zeolite play a positive correlation role in reducing radiation and improving the density of the fixed body.
[0097] By comparing Examples 1 and 4 with Comparative Example 6, it can be found that when the system does not contain activated carbon / white carbon black, the surface dose rate reduction effect decreases, which means that activated carbon / white carbon black plays a positive correlation role in reducing radiation.
[0098] By comparing Examples 1, 2, and 3, it can be found that when the water consumption fluctuates significantly, the various properties of the formula still meet the standards and the formula still has the conditions for engineering application, which means that the formula has an ideal envelope for the measurement error and system error of the engineering scale.
[0099] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0100] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
[0101] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A nuclear waste solidification material, comprising the following components in parts by weight: 40-50 parts of cementitious material; 20-60 parts of fine aggregate; 6-12 parts of mineral admixtures; 0.5-2.0 parts of admixtures; wherein the cementitious material is composed of low-heat silicate cement and barium silicate cement, the fine aggregate is composed of barite aggregate and quartz sand, the mineral admixture is composed of metakaolin, zeolite powder and a first material, and the first material is at least one of activated carbon and white carbon black; Among them, 40-50 parts of cementitious materials contain: 30-35 parts of low-heat silicate cement and 10-15 parts of barium silicate cement; Among them, 6-12 parts of mineral admixtures contain: 4-6 parts of metakaolin, 1-3 parts of zeolite powder; 1-3 parts of the first material; Among them, 20-60 parts of fine aggregate contain 10-50 parts of barite aggregate and 50-10 parts of quartz sand; The nuclear waste solidification material is used to solidify low and medium radioactive level solid waste.
2. The nuclear waste solidification material according to claim 1, wherein: The mesh size of the fine aggregate is 10-70.
3. The nuclear waste solidification material according to claim 1, wherein: 0.5-2.0 parts of admixtures contain: 0.3-1.0 parts of water reducing agent; 0.1-0.3 parts of defoaming agent; 0.1-0.3 parts of thickener.
4. The nuclear waste solidification material according to claim 3, wherein: The water reducer is a polycarboxylic acid water reducer; the defoamer is a solid particle type defoamer; and the thickener is cellulose ether.
5. The method for preparing the nuclear waste solidified material according to any one of claims 1 to 4, comprising: The components of the nuclear waste solidification material are mixed in proportion to obtain the nuclear waste solidification material.
6. A method for solidifying low- and medium-level radioactive solid wastes, comprising: The nuclear waste solidification material as described in any one of claims 1 to 4 is used to solidify low and medium radioactive level solid waste.
7. The method for solidifying low- and medium-level radioactive solid wastes as claimed in claim 6, comprising the following steps: Adding water to the nuclear waste solidification material according to any one of claims 1 to 4 at a water-to-material ratio of 0.11 to 0.17 by weight, and mixing well to obtain a nuclear waste solidification material mixture; The nuclear waste solidification material mixture is mixed evenly with the low and medium radioactive level solid wastes that need to be solidified, and poured, stored and disposed of according to the on-site construction requirements.