A magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate and a preparation method thereof
Patent Information
- Application Number
- CN202211561098.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-07
AI Technical Summary
[0010]1、2小时的高能球磨提高了时间成本和经济成本,增加了工艺环节和生产能耗;
[0045] 1. Compared with the existing technology, the present invention has a higher reversible hydrogen storage capacity, that is, the reversible hydrogen storage capacity is greater than 5.5wt.% at 300°C; at the same time, it has a higher hydrogen absorption and release rate, that is, under the conditions of 300°C and 3MPa The amount of hydrogen absorbed in 5 minutes is greater than 4. 0wt.%, the hydrogen release amount in 5 minutes under 300℃ and vacuum conditions is greater than 4.0wt.%; compared with the Mg-Ni-Y alloy in the reference example, the hydrogen absorption amount increased by 16.8% under the same hydrogen absorption and release time. The amount of hydrogen released increased by 25.7%.
Smart Images

Figure CN116121609B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of solid-state hydrogen storage, and in particular to a magnesium-based composite hydrogen storage material having high capacity and high hydrogen absorption and desorption rate and a preparation method thereof. Background Art
[0002] As a new energy source, hydrogen energy has the advantages of high energy density, clean combustion products, wide application, and abundant reserves. Metal hydride hydrogen storage technology is an important field of hydrogen energy. Among metal hydrides, magnesium-based hydrogen storage materials have a theoretical hydrogen storage capacity of up to 7.6wt.%, that is, the advantage of large hydrogen storage capacity. However, magnesium-based hydrogen storage alloys have problems such as high hydrogen absorption and desorption temperature and slow hydrogen absorption and desorption rate. The common solutions currently include: 1. Adding transition metals such as titanium, vanadium, and nickel or rare earth elements such as lanthanum, neodymium, yttrium, and cerium to magnesium-based hydrogen storage materials for alloying and preparing composite hydrogen storage materials; 2. Catalyst doping method; 3. Nano-sizing method.
[0003] Alloying is the most effective and commonly used method to improve the kinetics of hydrogen absorption and desorption through the preparation of composite hydrogen storage materials. The added alloying elements can form new magnesium-based hydrides or rare earth hydrides, thereby changing the hydrogen absorption and desorption reaction pathways of magnesium-based hydrogen storage alloys and helping to reduce the enthalpy change and activation energy of the hydrogen absorption and desorption reactions.
[0004] Among them, the Mg-Ni-Y hydrogen storage alloy has a magnesium-rich long-period stacking ordered (LPSO) phase, mainly including 14H and 18R. The LPSO phase is gradually decomposed when the hydrogen storage alloy absorbs hydrogen, and the rare earth hydride YH is evenly distributed in a long range. x and Mg 2 The formation of Ni achieves good catalytic effect and improves the hydrogen absorption and desorption kinetics of magnesium-based hydrogen storage materials, that is, Mg, Mg 2 Ni and YH x The phases together constitute magnesium-based composite hydrogen storage materials.
[0005] For example, prior art 1 (a Mg-Ni-Y hydrogen storage alloy with a multiphase eutectic structure and a preparation method thereof, CN110257651A[P].2019.) prepared a Mg-Ni-Y hydrogen storage alloy with a multiphase eutectic structure and a preparation method thereof, CN110257651A[P].2019. 2 Ni、MgYNi 4 The Mg-Ni-Y alloy has yttrium and magnesium content of 5-11 at.% and 76-87 at.%, respectively, and the LPSO phase fraction is 60-70 vol.%. The LPSO phase decomposes to form YH when the Mg-Ni-Y alloy absorbs hydrogen for the first time. x phase, and dispersed inside and on the surface of Mg particles, effectively improving the hydrogen absorption and desorption kinetics of the alloy. 2 Ni and YH xThe reversible hydrogen storage capacity of the magnesium-based composite hydrogen storage material composed of phases is 4.0wt.% at 300°C, and the hydrogen absorption within 3 minutes at 300°C and 3MPa is 3.57wt.%. However, this technology has the following problems:
[0006] 1. In order to increase the volume fraction of LPSO phase in magnesium-based hydrogen storage alloy, it is necessary to increase the amount of rare earth elements added and reduce the magnesium content, resulting in the magnesium content in the designed magnesium-based hydrogen storage alloy being lower than 90at.%, and the reversible hydrogen storage capacity of the finally prepared magnesium-based composite hydrogen storage material at 300°C is reduced to 5.0wt.%;
[0007] 2. The rare earth element content in the designed magnesium-based hydrogen storage alloy is greater than 5 at.%, which increases the raw material cost of alloy preparation.
[0008] In order to reduce the amount of rare earth elements added, nano-sized Mg grains prepared by high-energy ball milling can also increase the hydrogen absorption and desorption rate of Mg-Ni-Y powder.
[0009] For example, prior art 2 (a magnesium-based hydrogen storage alloy with a long period structure and a preparation method thereof, CN102337438B[P].2013.) prepared a Mg-containing 18R-type LPSO phase by induction melting, mechanical crushing and 2 hours of high-energy ball milling. 91.9 Ni 4.3 Y 3.8 Hydrogen storage alloy. The magnesium content of the Mg-Ni-Y alloy is higher than 90 at.%, and the alloy powder is subjected to high-energy ball milling for 2 hours after mechanical crushing to improve the activity of the alloy powder. The resulting magnesium-based composite hydrogen storage material has a hydrogen absorption capacity of 4.0 wt.% in 5 minutes and a hydrogen release capacity of 5.5 wt.% in 5 minutes at 300°C. However, this technology has the following problems:
[0010] 1. The 2-hour high-energy ball milling increases the time and economic costs, and increases the process steps and production energy consumption;
[0011] 2. After 20-30 cycles of hydrogen absorption and desorption, the Mg-Ni-Y powder obtained by ball milling is prone to Mg grain growth and particle agglomeration, resulting in a decrease in the hydrogen absorption and desorption rate of the material.
[0012] In order to overcome the problem of hydrogen absorption and desorption rate attenuation of Mg-Ni-Y powder, heavy rare earth elements can be added. The relative atomic mass of neodymium is 1.6 times that of yttrium, and it is more difficult to diffuse in Mg-Ni-RE hydrogen storage alloy. NdH formed after Mg-Ni-Nd hydrogen storage alloy absorbs hydrogen x The phase energy can play a pinning role on the Mg grain boundary, hindering the growth of Mg grains and avoiding particle agglomeration, thereby improving the hydrogen absorption and desorption cycle life of the Mg-based composite hydrogen storage material.
[0013] To this end, the research group of the present invention conducted preliminary work, and the prior art 3 (a method for designing a long-life Nd-Mg-Ni hydrogen storage alloy using a phase diagram, CN105861897A[P].2016.) prepared a Mg-Ni-Nd magnesium-based composite material by induction melting, annealing for 1-12 hours, mechanical crushing and hydrogen absorption and decomposition, wherein the magnesium content is 69-88at.%, and the neodymium content is 4-17at.%. The NdH formed by hydrogen absorption and decomposition of the Mg-Ni-Nd alloy x The hydrogen absorption and desorption cycle life of the magnesium-based composite material is effectively improved. 4 Mg 85 Ni 11 After 819 cycles of hydrogen absorption and desorption, the reversible hydrogen storage capacity of the hydrogen storage alloy at 300°C is 3.76wt.%, which is 79.2% of the maximum capacity. However, this technology has the following problems:
[0014] 1. Since neodymium is difficult to diffuse in Mg-Ni-Nd alloy, the Mg-Ni-Nd hydrogen storage alloy needs to be annealed for 1-12 hours during the preparation process to make the element distribution uniform, which increases the production energy consumption;
[0015] 2. Neodymium metal is expensive, about 3.5 times that of yttrium metal, and the neodymium content in the designed Mg-Ni-Nd hydrogen storage alloy is greater than 4at.%, which increases the preparation cost of the alloy;
[0016] 3. Neodymium has a large relative atomic mass of 144.2, so the prepared Nd 4 Mg 85 Ni 11 The maximum reversible hydrogen storage capacity of the hydrogen storage alloy at 300°C is only 4.74wt.%.
[0017] Therefore, when preparing magnesium-based composite hydrogen storage materials with both high capacity and high hydrogen absorption and desorption rates, it is necessary to solve the problem that the reversible hydrogen storage capacity of hydrogen storage alloys decreases when the amount of rare earth elements added is increased. When solving the above problems, the following problems also need to be solved:
[0018] 1. The magnesium content in the magnesium-based hydrogen storage alloy should be higher than 90 at.% to increase the reversible hydrogen storage capacity, the total content of rare earth elements should be lower than 3 at.% to reduce the raw material cost, and the volume fraction of the LPSO phase in the alloy should be greater than 40 vol.%;
[0019] 2. The magnesium-based composite hydrogen storage material achieves the high capacity target, i.e., the reversible hydrogen storage capacity is greater than 5.5wt.% at 300°C, while achieving the high hydrogen absorption and desorption rate target, i.e., the hydrogen absorption capacity is greater than 4.0wt.% in 5 minutes at 300°C and 3MPa, and the hydrogen desorption capacity is greater than 4.0wt.% in 5 minutes at 300°C and vacuum;
[0020] 3. Industrial production equipment can be used while avoiding the introduction of time-consuming and energy-consuming processes such as annealing heat treatment and ball milling. Summary of the invention
[0021] The purpose of the present invention is to provide a magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate and a preparation method thereof. The material is prepared by two steps: preparation of Mg-Ni-Y-Nd alloy and preparation of magnesium-based composite hydrogen storage material. The specific technology involves three links: induction melting, mechanical crushing and in-situ hydrogen absorption and decomposition, which reduces production costs and expands the scope of application.
[0022] In order to achieve the above-mentioned invention object, the present invention adopts the following inventive concept:
[0023] The present invention aims to solve the technical problems existing in the prior art by adopting the following methods:
[0024] According to the thermodynamic phase diagram database of Mg-Ni-Y-Nd system, the magnesium-rich corner of Mg-Ni-Y-Nd alloy, i.e., the magnesium content is higher than 90 at.%, the volume fraction of LPSO phase is greater than 40 vol.%, and there are Mg and Mg 2 The alloy composition range of Ni eutectic structure. 92 Ni 5 Y 2 The solidification path calculation of Nd alloy determined that the balanced solidification of the alloy helps to reduce the segregation of alloy components and the diffusion of rare earth elements, and increases the LPSO phase fraction in the alloy by 29.8 vol.%.
[0025] The designed Mg-Ni-Y-Nd alloy is prepared by induction melting and mechanical crushing. The prepared alloy contains LPSO phase and yttrium and neodymium elements are uniformly dissolved in the LPSO phase, avoiding the use of annealing heat treatment process to homogenize the alloy composition. At the same time, the lath-like LPSO phase divides the Mg matrix, and the NdH x The magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate is prepared by in-situ hydrogen absorption and decomposition of Mg-Ni-Y-Nd alloy, in which the Mg grain size is less than 50nm, avoiding the use of high-energy ball milling process to prepare nano-scale Mg grains; the LPSO phase containing yttrium and neodymium elements is uniformly dispersed and decomposed into rare earth hydride YH in a long range. x and NdH x , and as a catalyst to improve the hydrogen absorption and desorption kinetics of magnesium-based hydrogen storage materials.
[0026] According to the above inventive concept, the present invention adopts the following technical solution:
[0027] A magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate, wherein the magnesium-based composite hydrogen storage material is formed by in-situ hydrogen absorption and decomposition of a Mg-Ni-Y-Nd alloy, and comprises Mg, Mg 2 Ni and YH x and NdH x phase; the Mg-Ni-Y-Nd alloy composition is located at the magnesium-rich corner of the Mg-Ni-Y-Nd quaternary phase diagram, and the atomic percentage of the alloy composition is: Mg content is 90-95at.%, Ni content is 3-6at.%, Y content is 1-2at.%, Nd content is 1-2at.%, and the total content of Y and Nd does not exceed 3at.%; the Mg-Ni-Y-Nd alloy contains Mg, Mg 2 Ni and long-period stacking ordered LPSO phase;
[0028] The volume fraction of the LPSO phase containing yttrium and neodymium elements is 40-60 vol.%, and the configuration includes 14H and 18R types;
[0029] The LPSO phase containing yttrium and neodymium absorbs hydrogen in situ and decomposes to form YH with a grain size of 5-20 nm. x and NdH x phase, and is evenly dispersed inside and on the surface of Mg particles in a long range;
[0030] The Mg grain size in the magnesium-based composite hydrogen storage material is 30-50 nm;
[0031] The Mg in the Mg-Ni-Y-Nd alloy 2 The Ni phase is a needle-like phase, with Mg and Mg 2 Ni exists in the form of eutectic structure; the Mg 2 The volume fraction of the Ni phase is 6-15 vol.%, and the volume fraction of the Mg phase is 35-65 vol.%.
[0032] A method for preparing a magnesium-based composite hydrogen storage material having both high capacity and high hydrogen absorption and desorption rate comprises the following steps:
[0033] Step 1, preparation of Mg-Ni-Y-Nd alloy, with a certain atomic percentage of alloy components, repeatedly inverting raw material magnesium block, nickel block, yttrium block and neodymium block under certain conditions for induction melting, so as to obtain an ingot of Mg-Ni-Y-Nd alloy; then, after removing the surface oxide scale of the Mg-Ni-Y-Nd alloy ingot, mechanically crushing it under air conditions, and sieving it, so as to obtain a powder of Mg-Ni-Y-Nd alloy;
[0034] In step 1, the atomic percentages of the alloy components are: Mg content is 90-95 at.%, Ni content is 3-6 at.%, Y content is 1-2 at.%, Nd content is 1-2 at.%, and the total content of Y and Nd does not exceed 3 at.%;
[0035] The smelting conditions are as follows: the smelting temperature is 675-750°C, the smelting times are 3-5 times, after the smelting is completed, the alloy is cooled with the furnace at a cooling rate of 1-6°C / min, and when the alloy temperature is 300-400°C, the alloy is taken out and air-cooled to room temperature;
[0036] Step 2, preparation of magnesium-based composite hydrogen storage material, the powder of Mg-Ni-Y-Nd alloy obtained in step 1 is loaded into a closed reactor, after argon gas purge operation, hydrogen absorption treatment is performed under certain conditions, that is, in-situ hydrogen absorption and decomposition of Mg-Ni-Y-Nd alloy powder is completed, and then hydrogen desorption treatment is performed under certain conditions, that is, magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate of the present invention is obtained;
[0037] In step 2, the conditions for in-situ hydrogen absorption and decomposition are: under hydrogen conditions, the hydrogen absorption pressure is 4-6MPa, the hydrogen absorption temperature is 300-365°C, and the hydrogen absorption time is 3-6h; the conditions for hydrogen decomposition treatment are: under vacuum conditions, the hydrogen decomposition temperature is 300-365°C, and the hydrogen decomposition time is 0.5-1.5h.
[0038] In the application field of hydrogen storage materials, the reversible hydrogen storage capacity of the magnesium-based composite hydrogen storage material at 300°C is 5.5-6.1wt.%; the hydrogen absorption capacity of the magnesium-based composite hydrogen storage material at 300°C and 3MPa in 5 minutes is 4.0-5.0wt.%; and the hydrogen release capacity at 300°C and vacuum in 5 minutes is 4.0-5.0wt.%.
[0039] The technical effects of the present invention are as follows after experimental detection:
[0040] The XRD test results of Mg-Ni-Y-Nd alloy show that Mg-Ni-Y-Nd alloy contains Mg phase, Mg 2 Ni phase and LPSO phase, wherein the LPSO phase includes 18R type and 14H type. The SEM test results of Mg-Ni-Y-Nd alloy show that the LPSO phase in Mg-Ni-Y-Nd alloy is lath-shaped and divided by Mg matrix, and the volume fraction of LPSO phase is 40-60vol.%; Mg 2 The Ni phase is a needle-like phase, with Mg and Mg 2 Ni eutectic structure exists; in addition, the EDS point scanning test results of Mg-Ni-Y-Nd alloy show that the LPSO phase contains both yttrium and neodymium elements, and the atomic ratio of yttrium to neodymium is (4-6):1.
[0041] The XRD test results of the magnesium-based composite hydrogen storage material and the Rietveld method refinement results show that it contains Mg phase, Mg 2 Ni phase, YH x Phase and NdH x In addition, the Mg grain size in the magnesium-based composite hydrogen storage material is 30-50nm, YH x The grain size is 5-20nm, NdH x The grain size is 5-20nm. The LPSO phase in the Mg-Ni-Y-Nd alloy absorbs hydrogen in situ and decomposes to form Mg phase and Mg 2 Ni phase, YH x Phase and NdH x Phase, where YH x Phase and NdH x The phase is evenly dispersed in the long range and acts as a catalyst to improve the hydrogen absorption and desorption kinetics of magnesium-based hydrogen storage materials.
[0042] The PCT test results of the magnesium-based composite hydrogen storage material show that its reversible hydrogen storage capacity at 300°C is 5.5-6.1wt.%.
[0043] The results of the hydrogen absorption and desorption kinetics test of the magnesium-based composite hydrogen storage material show that at 300°C and 3MPa, the hydrogen absorption capacity is 4.0-5.0wt.% in 5 minutes; at 300°C and vacuum, the hydrogen desorption capacity is 4.0-5.0wt.% in 5 minutes.
[0044] Therefore, the above experimental detection shows that the present invention has the following advantages:
[0045] 1. Compared with the prior art, the present invention has a higher reversible hydrogen storage capacity, that is, the reversible hydrogen storage capacity at 300°C is greater than 5.5wt.%; at the same time, it has a higher hydrogen absorption and desorption rate, that is, the hydrogen absorption amount in 5 minutes under the conditions of 300°C and 3MPa is greater than 4.0wt.%, and the hydrogen desorption amount in 5 minutes under the conditions of 300°C and vacuum is greater than 4.0wt.%; compared with the Mg-Ni-Y alloy in the reference example, under the same hydrogen absorption and desorption time, the hydrogen absorption amount is increased by 16.8%, and the hydrogen desorption amount is increased by 25.7%.
[0046] 2. The magnesium-based composite hydrogen storage material designed and prepared by the present invention reduces the content of rare earth elements, and the total content does not exceed 3 at.%, which reduces the raw material cost by 10-40% compared with the prior art and is easy to promote commercially. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 The isothermal cross-section phase diagram and the vertical cross-section phase diagram of the Mg-Ni-Y-Nd alloy at 400°C with 0-2at.% neodymium addition are calculated for the present invention, wherein: Figure 1a is the isothermal cross-section phase diagram of Mg-Ni-Y alloy at 400℃. Figure 1 b is Mg (95-x) Ni 5 Y x Vertical cross-section phase diagram of alloy, Figure 1 c is the isothermal cross-section phase diagram of Mg-Ni-Y-Nd alloy at 400℃ when the neodymium content is 1at.%, Figure 1 d is Mg (94-x) Ni 5 Y x Vertical cross-section phase diagram of Nd alloy, Figure 1 e is the isothermal cross-section phase diagram of Mg-Ni-Y-Nd alloy at 400℃ when the neodymium content is 2at.%, Figure 1 f is Mg (93-x) Ni 5 Y x Nd 2 Phase diagram of vertical section of alloy;
[0048] Figure 2 Calculate Mg for the present invention 92 Ni 5 Y 2 Solidification path diagram of Nd hydrogen storage alloy, where: Figure 2 a is Mg 92 Ni 5 Y 2 Equilibrium solidification path diagram of Nd hydrogen storage alloy, Figure 2 b is Mg 92 Ni 5 Y 2 Non-equilibrium solidification path diagram of Nd hydrogen storage alloy;
[0049] Figure 3 The XRD patterns of the Mg-Ni-Y-Nd alloy powder and the magnesium-based composite hydrogen storage material prepared in the present invention are shown below. Figure 3 a is the XRD spectrum of the Mg-Ni-Y-Nd alloy powder prepared in Example 1 and the Mg-Ni-Y-Nd alloy powder prepared in Comparative Example 1, Figure 3 b is #1-Y prepared in Example 1 2 XRD patterns of Nd in hydrogen absorption and desorption states;
[0050] Figure 4 is a SEM image of the microstructure of the Mg-Ni-Y-Nd alloy ingot in Example 1 of the present invention;
[0051] Figure 5 The PCT curves of the magnesium-based composite hydrogen storage materials prepared in Example 1 and Comparative Example 1 of the present invention at 300° C.
[0052] Figure 6The graph is a hydrogen absorption kinetics curve of the magnesium-based composite hydrogen storage material prepared in Example 1 of the present invention and Comparative Example 1 at 300° C. and 3-5 MPa;
[0053] Figure 7 The graph is a hydrogen desorption kinetics curve of the magnesium-based composite hydrogen storage material prepared in Example 1 of the present invention and Comparative Example 1 at 300° C. and vacuum conditions. DETAILED DESCRIPTION
[0054] The present invention is further described in detail through embodiments and in conjunction with the accompanying drawings, but the present invention is not limited thereto.
[0055] Since there is no published content related to the thermodynamic phase diagram of the Mg-Ni-Y-Nd system, the inventors of the present invention have experimented and determined the phase equilibrium relationship of the Mg-Ni-Y-Nd system in order to obtain the types and volume fractions of the phases in the Mg-Ni-Y-Nd alloy, and constructed and disclosed for the first time in this invention some relevant data in the thermodynamic phase diagram database of the Mg-Ni-Y-Nd system, namely Figure 1 a. Figure 1 c and Figure 1 e.
[0056] Then, based on the constructed Mg-Ni-Y-Nd system thermodynamic phase diagram database, the following is obtained by thermodynamic calculation: Figure 1 a. Figure 1 c and Figure 1 The reference example, embodiment 1-2 and comparative example 1-2 shown in e correspond to the isothermal cross-section phase diagram of the alloy at 400°C; and the Mg and Mg in the Mg-Ni-Y-Nd alloy are calculated. 2 The phase fractions of Ni and LPSO are shown in Table 1 and Figure 1 b. Figure 1 d and Figure 1 f.
[0057] In order to clarify the content of Mg, Mg 2 The phase fractions of Ni and LPSO phases were calculated based on the isothermal cross-section phase diagram of the corresponding alloy at 400°C. The results are shown in Table 1.
[0058] Table 1 Phase types and volume fractions in Mg-Ni-Y-Nd alloy
[0059]
[0060] Embodiment 1:
[0061] A method for preparing a magnesium-based composite hydrogen storage material having both high capacity and high hydrogen absorption and desorption rate, specifically comprising the following steps:
[0062] Step 1, preparation of Mg-Ni-Y-Nd alloy, with the atomic percentage of alloy components as follows: Mg content is 92at.%, Ni content is 5at.%, Y content is 2at.%, Nd content is 1at.%, raw materials magnesium block, nickel block, yttrium block and neodymium block are repeatedly inverted for induction melting at a melting temperature of 700°C and melting times of 5 times, after melting, they are furnace cooled at a cooling rate of 3°C / min., when the alloy temperature is 400°C, the alloy is taken out and air-cooled to room temperature to obtain an ingot of Mg-Ni-Y-Nd alloy; then, after removing the surface oxide scale of the Mg-Ni-Y-Nd alloy ingot, it is mechanically crushed under air conditions, and sieved at 200 mesh conditions to obtain a powder of Mg-Ni-Y-Nd alloy;
[0063] Step 2, preparation of magnesium-based composite hydrogen storage material, the powder of Mg-Ni-Y-Nd alloy obtained in step 1 is loaded into a closed reactor, and after argon gas purge operation is performed 3 times, hydrogen absorption treatment is performed under hydrogen conditions at a hydrogen absorption pressure of 5MPa, a hydrogen absorption temperature of 350°C, and a hydrogen absorption time of 4h, that is, the in-situ hydrogen absorption and decomposition of the Mg-Ni-Y-Nd alloy powder is completed, and then hydrogen decomposition treatment is performed under vacuum conditions at a hydrogen decomposition temperature of 350°C and a hydrogen decomposition time of 0.5h, so as to obtain the magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and decomposition rate of the present invention, which is named #1-Y 2 Nd.
[0064] In order to verify the phase types and mass fractions of the Mg-Ni-Y-Nd alloy, as well as the phase changes during the preparation process, the Mg-Ni-Y-Nd alloy obtained in step 1 and the #1-Y 2 Nd was subjected to XRD test and Rietveld method refinement. At the same time, the ingot of Mg-Ni-Y-Nd alloy obtained in step 1 was subjected to SEM test and EDS test to determine the morphology and volume fraction of each phase in the Mg-Ni-Y-Nd alloy.
[0065] The XRD test results of Mg-Ni-Y-Nd alloy and the mass fraction of each phase obtained by Rietveld method are shown in the figure. Figure 3 As shown in a and Table 2, the Mg-Ni-Y-Nd alloy contains Mg phase, Mg 2 Ni phase and LPSO phase, wherein the LPSO phase includes 18R type and 14H type.
[0066] The SEM test results of Mg-Ni-Y-Nd alloy and the volume fraction and average size of each phase are shown in Figure 4 As shown in Table 2, the LPSO phase is lath-shaped and divided by the Mg matrix; Mg 2 The Ni phase is a needle-like phase, with Mg and Mg2 Ni eutectic structure exists; in addition, the EDS point scanning test results of Mg-Ni-Y-Nd alloy show that the LPSO phase contains both yttrium and neodymium elements, among which the composition of 18R type LPSO phase is 87.1at.% Mg, 6.0at.% Ni, 5.6at.% Y and 1.3at.% Nd, and the atomic ratio of yttrium to neodymium is 4.3:1; the composition of 14H type LPSO phase is 90.1at.% Mg, 3.8at.% Ni, 5.2at.% Y and 0.9at.% Nd, and the atomic ratio of yttrium to neodymium is 5.8:1.
[0067] Table 2 Phase fraction and average size in Mg-Ni-Y-Nd alloy
[0068]
[0069] The following conclusions can be drawn from the above XRD and EDS test results: the volume fraction of LPSO phase in Mg-Ni-Y-Nd alloy is 40-60 vol.%; and yttrium and neodymium are uniformly dissolved in LPSO phase of Mg-Ni-Y-Nd alloy; in addition, due to the lamellar LPSO phase segmenting the Mg matrix, the NdH x Phase limits the growth of Mg grains.
[0070] #1-Y 2 The XRD test results of Nd are as follows Figure 3 As shown in b, #1-Y 2 Nd contains Mg phase, Mg 2 Ni phase, YH x Phase and NdH x phase; the corresponding mass fractions of each substance are: the mass fraction of Mg phase is 71.9wt.%, Mg 2 The mass fraction of Ni phase is 16.9wt.%, YH x The mass fraction of the phase is 7.4wt.%, NdH x The mass fraction of the phase is 3.9wt.%, and #1-Y 2 The average grain size of Mg in Nd is 44.9nm, YH x The average grain size is 12.7nm, NdH x The average grain size is 7.3 nm, thus avoiding the introduction of high-energy ball milling process that consumes a lot of energy and time to prepare nano-sized Mg grains.
[0071] The Mg-Ni-Y-Nd alloy and #1-Y 2 Nd, it can be seen that the LPSO phase in the Mg-Ni-Y-Nd alloy absorbs hydrogen in situ and decomposes to form Mg phase and Mg2 Ni phase, YH x Phase and NdH x Phase, where YH x Phase and NdH x The phase is evenly dispersed in the long range and acts as a catalyst to improve the hydrogen absorption and desorption kinetics of magnesium-based hydrogen storage materials; #1-Y 2 Mg, YH in Nd x and NdH x It has nano-scale grain size, with Mg grain size of 30-50nm, YH x and NdH x The grain size is 5-20nm.
[0072] To prove #1-Y 2 The hydrogen storage capacity of Nd was tested by PCT. The test results are as follows Figure 5 As shown, the reversible hydrogen storage capacity at 300 °C is 6.02 wt.%.
[0073] To prove #1-Y 2 The absorption and desorption rate of Nd was tested for the kinetics of absorption and desorption of hydrogen. Figure 6 and Figure 7 As shown, at 300°C and 3 MPa, the hydrogen absorption amount in 1 minute is 4.15wt.%, and the hydrogen absorption amount in 5 minutes is 4.64wt.%; at 300°C and vacuum, the hydrogen release amount in 5 minutes is 4.01wt.%.
[0074] The above-mentioned hydrogen absorption and desorption kinetic test results can prove that the REH generated by the LPSO phase containing yttrium and neodymium elements after in-situ hydrogen absorption and decomposition x The phase can effectively catalyze the hydrogen absorption and desorption reactions of magnesium-based composite hydrogen storage materials.
[0075] In order to prove the effect of adding neodymium on magnesium-based composite hydrogen storage materials, a reference ratio is provided. The magnesium-based composite hydrogen storage material without neodymium is named #0-Y 2 .
[0076] Reference ratio
[0077] A magnesium-based composite hydrogen storage material without adding neodymium, wherein the steps not specifically described are the same as those in Example 1, except that: in the atomic percentage composition of the alloy components in step 1, the Ni and Y contents are kept unchanged, and no Nd element is added. In order to control the variables, the Mg content is changed from 92 at.% to 93 at.%, and after in-situ hydrogen absorption and decomposition, the final material obtained is #0-Y without adding neodymium. 2 .
[0078] #0-Y 2The PCT test results showed that the reversible hydrogen storage capacity at 300 °C was 6.17 wt.%.
[0079] #0-Y 2 The results of hydrogen absorption and desorption kinetics test show that at 300℃ and 3MPa, the hydrogen absorption amount is 3.97wt.% in 5 minutes; at 300℃ and vacuum, the hydrogen desorption amount is 3.19wt.% in 5 minutes.
[0080] By comparing Example 1 with the reference example, it can be seen that the reversible hydrogen storage capacity of the magnesium-based composite hydrogen storage material without the addition of neodymium element at 300°C only increased by 0.15wt.%; while at 300°C and 3MPa, the hydrogen absorption amount in 5 minutes decreased by 0.67wt.%; at 300°C and vacuum, the hydrogen release amount in 5 minutes decreased by 0.82wt.%.
[0081] The test results show that the magnesium-based composite hydrogen storage material with the addition of neodymium has higher hydrogen absorption and desorption kinetics. The reasons for this result are analyzed as follows: Figure 1 As shown in Table 1, the LPSO phase fraction in the Mg-Ni-Y alloy ingot without adding neodymium element obtained in step 1 is reduced by 25 vol.%. 2 With less REH x particles, which in turn leads to a decrease in the kinetics of hydrogen absorption and desorption.
[0082] In order to demonstrate the influence of the preparation process on the magnesium-based composite hydrogen storage material, comparative example 1 is provided, in which the magnesium-based composite hydrogen storage material is prepared by annealing + quenching treatment instead of air cooling, and is named #2-Y 2 Nd.
[0083] Comparative Example 1
[0084] A magnesium-based composite hydrogen storage material using annealing + quenching treatment, the steps not specifically described are the same as those in Example 1, except that: when the furnace is cooled to 400°C in step 1, air cooling is not performed, but annealing + quenching treatment is performed. The specific method is to perform annealing treatment under the conditions of annealing temperature of 400°C and annealing time of 24h. After the annealing treatment is completed, the sample is quenched in an ice-water mixture. After in-situ hydrogen absorption and decomposition, the final material obtained is #2-Y treated by annealing + quenching. 2 Nd.
[0085] #2-Y 2 The PCT test results of Nd are as follows Figure 5 As shown, the reversible hydrogen storage capacity at 300 °C is 5.76 wt.%.
[0086] #2-Y 2 The results of the Nd hydrogen absorption and desorption kinetics test are as follows: Figure 6 and Figure 7 As shown, at 300°C and 3 MPa, the amount of hydrogen absorbed in 5 minutes is 3.99 wt.%; at 300°C and vacuum, the amount of hydrogen released in 5 minutes is 3.21 wt.%.
[0087] Comparison between Comparative Example 1 and Example 1 shows that the annealed and quenched #2-Y 2 The reversible hydrogen storage capacity of Nd at 300°C decreased by 0.65wt.%, while at 300°C and 3MPa, the hydrogen absorption in 5 minutes decreased by 0.65wt.%, and at 300°C and vacuum, the hydrogen desorption in 5 minutes decreased by 0.80wt.%.
[0088] The test results show that the annealed + quenched #2-Y 2 Nd has lower hydrogen absorption and desorption kinetics. The reasons for this result are analyzed as follows: Figure 3 It can be seen from Figure 1 that the LPSO phase in the Mg-Ni-Y-Nd alloy powder that has not been annealed + quenched has a broader diffraction peak, which is specifically manifested in the diffraction peaks of 2θ of 33.2° and 35.6°. This shows that after the annealing + quenching treatment of the Mg-Ni-Y-Nd alloy, the lattice distortion in the LPSO phase is weakened, the hydrogen atom diffusion channel is reduced, and the hydrogen absorption and desorption kinetics are reduced.
[0089] In order to demonstrate the influence of the alloy components, i.e., the addition amount of yttrium and neodymium elements, on the magnesium-based composite hydrogen storage material, Example 2 and Comparative Example 2 are provided, wherein:
[0090] The alloy composition atomic percentages of Example 2 are: Mg content is 92 at.%, Ni content is 5 at.%, Y content is 1 at.%, Nd content is 2 at.%, and the prepared magnesium-based composite hydrogen storage material is named #3-YNd 2 ;
[0091] The alloy composition atomic percentages of Comparative Example 2 are: Mg content is 91 at.%, Ni content is 5 at.%, Y content is 2 at.%, Nd content is 2 at.%, and the prepared magnesium-based composite hydrogen storage material is named #4-Y 2 Nd 2 .
[0092] Example 2
[0093] A magnesium-based composite hydrogen storage material having a Y content of 1 at.% and a Nd content of 2 at.%, wherein the steps not specifically described are the same as those in Example 1, except that: in the atomic percentage composition of the alloy components in step 1, the Mg and Ni contents are kept unchanged, the Y content is reduced from 2 at.% to 1 at.%, and the Nd content is increased from 1 at.% to 2 at.%, and after in-situ hydrogen absorption and decomposition, the final material obtained is #3-YNd having a Y content of 1 at.% and a Nd content of 2 at.%. 2 .
[0094] #3-YNd 2 The PCT test results showed that the reversible hydrogen storage capacity at 300 °C was 5.75 wt.%.
[0095] #3-YNd 2 The results of hydrogen absorption and desorption kinetic tests show that at 300°C and 3MPa, the hydrogen absorption amount is 4.56wt.% in 5 minutes; at 300°C and vacuum, the hydrogen desorption amount is 4.01wt.% in 5 minutes.
[0096] The test results show that #3-YNd with 1% Y and 2% Nd 2 It can also achieve the goals of high capacity and high hydrogen absorption and desorption rate, that is, the magnesium-based composite hydrogen storage material with a total content of Y and Nd not exceeding 3% can meet the requirements of a reversible hydrogen storage capacity greater than 5.5wt.% at 300°C, a hydrogen absorption capacity greater than 4.0wt.% in 5 minutes under conditions of 300°C and 3MPa, and a hydrogen desorption capacity greater than 4.0wt.% in 5 minutes under conditions of 300°C and vacuum.
[0097] Comparative Example 2
[0098] A magnesium-based composite hydrogen storage material having a Y content of 2 at.% and a Nd content of 2 at.%, wherein the steps not specifically described are the same as those in Example 1, except that: in the atomic percentage composition of the alloy components in step 1, the Ni and Y contents are kept unchanged, and the Nd content is increased from 1 at.% to 2 at.%, and in order to control the variables, the Mg content is changed from 92 at.% to 91 at.%, and after in-situ hydrogen absorption and decomposition, the final material obtained is #4-Y having a Y content of 2 at.% and a Nd content of 2 at.%. 2 Nd 2 .
[0099] #4-Y 2 Nd 2 The PCT test results showed that the reversible hydrogen storage capacity at 300 °C was 5.37 wt.%.
[0100] #4-Y 2 Nd 2The results of hydrogen absorption and desorption kinetics test show that at 300℃ and 3MPa, the hydrogen absorption amount is 4.55wt.% in 5 minutes; at 300℃ and vacuum, the hydrogen desorption amount is 3.89wt.% in 5 minutes.
[0101] Comparing Comparative Example 2 with Example 1, it can be seen that #4-Y with a Y content of 2% and a Nd content of 2% 2 Nd 2 The reversible hydrogen storage capacity at 300°C decreased by 0.65wt.%, while at 300°C and 3MPa, the hydrogen absorption in 5 minutes decreased by 0.08wt.%, and at 300°C and vacuum, the hydrogen desorption in 5 minutes decreased by 0.12wt.%.
[0102] The test results show that when the total content of rare earth elements in the magnesium-based composite hydrogen storage material is greater than 3%, the reversible hydrogen storage capacity of the material at 300°C will be lower than 5.5wt.%. The reasons for this result are analyzed as follows: Figure 1 As shown in Table 1, when the Y content in the Mg-Ni-Y-Nd alloy is 2 at.% and the Nd content is 2 at.%, only Mg 2 Ni phase and LPSO phase, but lack of Mg phase, which leads to a decrease in the reversible hydrogen storage capacity of the magnesium-based composite hydrogen storage material.
[0103] By comparing and analyzing Examples 1-2, Reference Examples and Comparative Examples 1-2, the following conclusions can be drawn:
[0104] 1. The reversible hydrogen storage capacity of the magnesium-based composite hydrogen storage material shows a downward trend with the increase of the content of yttrium and neodymium. When the total content of yttrium and neodymium is greater than 3at.%, the reversible hydrogen storage capacity of the magnesium-based composite hydrogen storage material at 300°C is less than 5.5wt.%;
[0105] 2. The hydrogen absorption and desorption kinetics of the magnesium-based composite hydrogen storage material do not show an obvious correlation with the yttrium and neodymium content. Only through a limited number of attempts on the yttrium and neodymium content, it is impossible to predict that the highest hydrogen absorption and desorption kinetics can be obtained when the yttrium content is 2at.% and the neodymium content is 1at.%, that is, the hydrogen absorption amount is greater than 4.0wt.% in 5 minutes under 300℃ and 3MPa conditions, and the hydrogen desorption amount is greater than 4.0wt.% in 5 minutes under 300℃ and vacuum conditions.
[0106] 3. The preparation process of magnesium-based composite hydrogen storage materials has a significant impact on their hydrogen absorption and desorption kinetics. Adding annealing + quenching process will result in a 0.65wt.% decrease in hydrogen absorption in 5 minutes at 300℃ and 3MPa; and a 0.80wt.% decrease in hydrogen desorption in 5 minutes at 300℃ and vacuum.
[0107] Therefore, according to the above analysis, it can be seen that the present invention can achieve significant technical effect improvement only by calculating the phase diagram and using the method of preparing magnesium-based composite hydrogen storage materials by induction melting, mechanical crushing and in-situ hydrogen absorption and decomposition.
[0108] In summary, the above embodiment of the present invention provides a magnesium-based composite hydrogen storage material with both high capacity and high hydrogen absorption and desorption rate and a preparation method thereof, and uses phase diagram calculation to guide component design, and prepares materials according to the atomic percentage of alloy components: Mg content is 90-95at.%, Ni content is 3-6%, Y content is 1-2at.%, Nd content is 1-2at.%, and the total content of Y and Nd does not exceed 3at.%, and after induction melting, mechanical crushing and in-situ hydrogen absorption and decomposition, a magnesium-based composite hydrogen storage material with both high capacity and high hydrogen absorption and desorption rate is obtained. The magnesium-based composite hydrogen storage material prepared by the present invention generates REH in situ in the form of in-situ hydrogen absorption and decomposition of LPSO phase. x Particles, when the yttrium content is 2at.% and the neodymium content is 1at.%, the reversible hydrogen storage capacity of the magnesium-based composite hydrogen storage material at 300°C is 6.02wt.%, while the hydrogen absorption capacity at 300°C and 3MPa in 3 minutes is 4.64wt.%, and the hydrogen release capacity at 300°C and vacuum in 5 minutes is 4.01wt.%, which reduces the production cost and has broad application prospects.
[0109] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made according to the purpose of the invention of the present invention. Any changes, modifications, substitutions, combinations or simplifications made according to the spirit and principle of the technical solution of the present invention should be equivalent replacement methods. As long as they meet the purpose of the invention of the present invention and do not deviate from the technical principles and inventive concepts of the magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate and the preparation method thereof, they all belong to the protection scope of the present invention.
Claims
1. A magnesium-based composite hydrogen storage material having both high capacity and high hydrogen absorption and desorption rate, characterized in that: The magnesium-based composite hydrogen storage material is formed by in-situ hydrogen absorption and decomposition of a Mg-Ni-Y-Nd alloy, and comprises Mg, Mg2Ni and YH x and NdH x phase; the Mg-Ni-Y-Nd alloy composition is located at the magnesium-rich corner of the Mg-Ni-Y-Nd quaternary phase diagram, and the atomic percentages of the alloy components are: Mg content is 90-95at.%, Ni content is 3-6at.%, Y content is 1-2at.%, Nd content is 1-2at.%, and the total content of Y and Nd does not exceed 3at.%; the Mg-Ni-Y-Nd alloy contains Mg, Mg2Ni and a long-period stacking ordered LPSO phase; the volume fraction of the LPSO phase is 40-60vol.%, and the configuration includes 14H and 18R types.
2. The magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate according to claim 1, characterized in that: The LPSO phase absorbs hydrogen in situ and decomposes to form YH with a grain size of 5-20 nm. x and NdH x phase, and is evenly dispersed inside and on the surface of Mg particles in a long range.
3. The magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate according to claim 1, characterized in that: The Mg grain size in the magnesium-based composite hydrogen storage material is 30-50 nm.
4. The magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate according to claim 1, characterized in that: The Mg2Ni phase in the Mg-Ni-Y-Nd alloy is a needle-shaped phase and exists in the form of a eutectic structure of Mg and Mg2Ni; the volume fraction of the Mg2Ni phase is 6-15 vol.%, and the volume fraction of the Mg phase is 35-65 vol.%.
5. A method for preparing a magnesium-based composite hydrogen storage material having both high capacity and high hydrogen absorption and desorption rate, characterized in that The following steps are involved: Step 1, preparation of Mg-Ni-Y-Nd alloy, with a certain atomic percentage of alloy components, repeatedly inverting raw material magnesium block, nickel block, yttrium block and neodymium block under certain conditions for induction melting, to obtain an ingot of Mg-Ni-Y-Nd alloy; then, after removing the surface oxide scale of the Mg-Ni-Y-Nd alloy ingot, mechanically crushing it under air conditions, and sieving it to obtain a powder of Mg-Ni-Y-Nd alloy; In step 1, the atomic percentages of the alloy components are: Mg content is 90-95 at.%, Ni content is 3-6 at.%, Y content is 1-2 at.%, Nd content is 1-2 at.%, and the total content of Y and Nd does not exceed 3 at.%; The smelting conditions are as follows: the smelting temperature is 675-750°C, the smelting times are 3-5 times, after the smelting is completed, the alloy is cooled with the furnace at a cooling rate of 1-6°C / min, and when the alloy temperature is 300-400°C, the alloy is taken out and air-cooled to room temperature; Step 2, preparation of a magnesium-based composite hydrogen storage material, wherein the powder of the Mg-Ni-Y-Nd alloy obtained in step 1 is loaded into a closed reactor, subjected to an argon gas purge operation, and then subjected to a hydrogen absorption treatment under certain conditions, i.e., the in-situ hydrogen absorption and decomposition of the Mg-Ni-Y-Nd alloy powder is completed, and then subjected to a hydrogen release treatment under certain conditions, to obtain a magnesium-based composite hydrogen storage material having both high capacity and high hydrogen absorption and desorption rate of the present invention; In step 2, the conditions for in-situ hydrogen absorption and decomposition are: under hydrogen conditions, the hydrogen absorption pressure is 4-6MPa, the hydrogen absorption temperature is 300-365°C, and the hydrogen absorption time is 3-6h; the conditions for hydrogen decomposition treatment are: under vacuum conditions, the hydrogen decomposition temperature is 300-365°C, and the hydrogen decomposition time is 0.5-1.5h.
6. The magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate according to claim 1, characterized in that: As an application in the field of hydrogen storage materials, the reversible hydrogen storage capacity at 300°C is 5.5-6.1wt.%.
7. The magnesium-based composite hydrogen storage material with high capacity and high hydrogen absorption and desorption rate according to claim 1, characterized in that: As an application in the field of hydrogen storage materials, at 300°C and 3MPa, the hydrogen absorption capacity is 4.0-5.0wt.% in 5 minutes; at 300°C and vacuum, the hydrogen release capacity is 4.0-5.0wt.% in 5 minutes.