Magnesium-zirconium master alloy and preparation method thereof

By melting magnesium under high-frequency induction and alternately stirring under low-frequency induction conditions, the problems of high energy consumption and component segregation in the preparation of magnesium-zirconium master alloy are solved, and the effects of fine zirconium particle size, dispersed distribution and low environmental pollution are achieved.

CN116121610BActive Publication Date: 2024-10-18HUNAN RARE EARTH METAL MATERIAL RES INST
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211725589.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-18
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

The existing traditional preparation method of magnesium-zirconium master alloy has problems such as high energy consumption, environmental protection problems, coarse zirconium particles and easy agglomeration, leading to serious component segregation and slag inclusion.

Method used

After high-frequency induction is used to smelt magnesium, alternating stirring is carried out under low-frequency induction conditions, including stirring in different directions, to ensure fine and dispersed distribution of zirconium particles, and to reduce component segregation and inclusions through fixed-point casting.

Benefits of technology

A magnesium-zirconium master alloy with fine zirconium particle size, dispersed distribution, smaller component segregation, and fewer inclusions has been achieved, with a simple preparation process and less environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116121610B_ABST
    Figure CN116121610B_ABST
Patent Text Reader

Abstract

The present application relates to a magnesium-zirconium master alloy and a preparation method thereof, comprising the following steps: melting metal magnesium under high-frequency induction conditions to obtain a first melt; adding metal zirconium to the first melt and performing alternating stirring under low-frequency induction conditions to obtain a second melt; the alternating stirring includes first stirring, second stirring and third stirring; the direction of the first stirring is that the upper melt flows upward from the center and downward from the side wall, and the lower melt flows upward from the side wall and downward from the center; the direction of the second stirring is that the melt flows upward from the side wall and downward from the center; the direction of the third stirring is that the melt flows upward from the center and downward from the side wall; under the action of the third stirring, the second melt is cast at a fixed point to obtain a magnesium-zirconium master alloy. The preparation method of the magnesium-zirconium master alloy makes the zirconium particles in the casted magnesium-zirconium master alloy fine, the zirconium particles dispersed, the zirconium content is high, the component segregation is small, and the inclusions are less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of alloys, and in particular to a magnesium-zirconium master alloy and a preparation method thereof. Background Art

[0002] Compared with physical field refinement, dynamic grain recrystallization and other methods, the addition of 0.5wt% zirconium particles can reduce the grain size of magnesium alloy from 100μm and above to less than 50μm without destroying its grain boundary precipitation, thereby effectively improving the performance of magnesium devices.

[0003] Since the solubility of zirconium in magnesium is very low, when the zirconium content exceeds 0.6wt%, the mechanical mixing of magnesium and zirconium will cause segregation problems. The traditional preparation method of magnesium-zirconium master alloy is to use magnesium to reduce potassium zirconate, but this method has a high reduction temperature (900℃~1000℃) and high energy consumption; the molten salt volatilizes seriously, and the environmental protection problem is prominent; the zirconium particles are coarse and easy to agglomerate and settle, resulting in serious component segregation and easy to produce slag inclusions.

[0004] Therefore, it is of great significance to provide a magnesium-zirconium master alloy with smaller component segregation. Summary of the invention

[0005] Based on this, the present application provides a magnesium-zirconium master alloy with fine zirconium particle size, dispersed zirconium particles, and small component segregation, and a preparation method thereof.

[0006] The technical solution of this application to solve the above technical problems is as follows.

[0007] A method for preparing a magnesium-zirconium master alloy comprises the following steps:

[0008] Melting metal magnesium under high-frequency induction conditions to obtain a first melt;

[0009] Adding metal zirconium to the first melt, and performing alternating stirring under low-frequency induction conditions to obtain a second melt; the alternating stirring includes first stirring, second stirring and third stirring; the first stirring direction is that the upper melt flows upward from the center and downward from the side walls, and the lower melt flows upward from the side walls and downward from the center; the second stirring direction is that the melt flows upward from the side walls and downward from the center; the third stirring direction is that the melt flows upward from the center and downward from the side walls;

[0010] Under the action of the third stirring, the second melt is cast at a fixed point to obtain a magnesium-zirconium master alloy.

[0011] In some of the embodiments, in the method for preparing the magnesium-zirconium master alloy, the alternating stirring is to perform the third stirring and the second stirring in sequence, and then cyclically perform the first stirring, the second stirring and the third stirring.

[0012] In some of the embodiments, in the method for preparing the magnesium-zirconium master alloy, the alternating stirring is to first perform the second stirring, and then cyclically perform the first stirring, the second stirring and the third stirring.

[0013] In some of the embodiments, in the method for preparing the magnesium-zirconium master alloy, the alternating stirring is to first perform the third stirring, and then cyclically perform the first stirring, the second stirring and the third stirring.

[0014] In some of the embodiments, in the method for preparing the magnesium-zirconium master alloy, the alternating stirring is cyclically performing the first stirring, the second stirring and the third stirring.

[0015] In some of the embodiments, in the method for preparing the magnesium-zirconium master alloy, the total time of the alternating stirring is 0.5 h to 3 h.

[0016] In some of the embodiments, in the method for preparing the magnesium-zirconium master alloy, the frequency of the high-frequency induction is 1000 Hz to 4000 Hz, and the frequency of the low-frequency induction is 20 Hz to 200 Hz.

[0017] In some embodiments, in the method for preparing the magnesium-zirconium master alloy, the smelting is performed at a first temperature, the alternating stirring is performed at a second temperature, and the first temperature and the second temperature are independently 700° C. to 800° C.

[0018] In some of the embodiments, in the method for preparing the magnesium-zirconium master alloy, the fixed-point casting is performed at a third temperature, and the third temperature is 720°C to 780°C.

[0019] In some of the embodiments, in the method for preparing the magnesium-zirconium master alloy, the step of preparing the magnesium-zirconium master alloy is carried out in a three-phase induction atmosphere furnace, using a mixed atmosphere of SF6 and CO2 for protection, and the melting power of the three-phase induction atmosphere furnace is 20kW to 300kW.

[0020] In some of the embodiments, in the method for preparing the magnesium-zirconium master alloy, before the step of adding metal zirconium into the first melt, the method further includes the step of depassivating the surface of the metal zirconium.

[0021] In some embodiments, in the method for preparing the magnesium-zirconium master alloy, the metal zirconium accounts for 0.1 wt% to 40 wt% of the magnesium-zirconium master alloy.

[0022] The present application also provides a magnesium-zirconium master alloy, which is prepared by the above-mentioned method for preparing the magnesium-zirconium master alloy.

[0023] Compared with the prior art, the preparation method of the magnesium-zirconium master alloy of the present application has the following beneficial effects:

[0024] In the preparation method of the magnesium-zirconium master alloy, metal magnesium is smelted under high-frequency induction conditions, and then metal zirconium is added and stirred alternately in different directions under low-frequency induction conditions. The low-frequency induction method with adjustable phase difference ensures that the stirring force intensity and the melt flow direction are controllable. Further, fixed-point casting is performed under the action of a specific stirring method, so that the zirconium particles in the obtained magnesium-zirconium master alloy are fine, the zirconium particles are dispersed, the zirconium content is high, the component segregation is small, and the inclusions are less. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0026] Figure 1 is a schematic diagram of a first stirring mode;

[0027] Figure 2 is a schematic diagram of the second stirring mode;

[0028] Figure 3 is a schematic diagram of the third stirring mode;

[0029] Figure 4 This is an overall photograph of the magnesium-zirconium alloy ingot prepared in Example 1;

[0030] Figure 5 This is a cross-sectional photograph of the magnesium-zirconium alloy ingot prepared in Example 1;

[0031] Figure 6 This is a 100-fold microstructure diagram of the magnesium-zirconium alloy ingot obtained in Example 1;

[0032] Figure 7 This is a 500-fold microstructure diagram of the magnesium-zirconium alloy ingot obtained in Example 1;

[0033] Figure 8 This is an overall photograph of the magnesium-zirconium alloy ingot prepared in Comparative Example 1;

[0034] Fig. 9 This is a cross-sectional photograph of the magnesium-zirconium alloy ingot prepared in Comparative Example 1;

[0035] Fig.10 The microstructure diagram of the magnesium-zirconium alloy ingot prepared in Comparative Example 1 is 100 times larger;

[0036] Fig.11 This is a 500-fold microstructure diagram of the magnesium-zirconium alloy ingot prepared in Comparative Example 1;

[0037] Fig.12 This is an overall photograph of the magnesium-zirconium alloy ingot prepared in Comparative Example 2;

[0038] Fig.13 This is a cross-sectional photograph of the magnesium-zirconium alloy ingot prepared in Comparative Example 2;

[0039] Fig.14 This is a 100-fold microstructure diagram of the magnesium-zirconium alloy ingot prepared in Comparative Example 2;

[0040] Fig.15 The microstructure diagram of the magnesium-zirconium alloy ingot obtained in Comparative Example 2 is 500 times larger;

[0041] Fig.16 is a statistical diagram of the size of zirconium particles in the magnesium-zirconium alloy ingot prepared in Example 1;

[0042] Fig.17 This is a statistical diagram of the size of zirconium particles in the magnesium-zirconium alloy ingot prepared in Comparative Example 1. DETAILED DESCRIPTION

[0043] The technical solution of the present application is further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. It should be understood that the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0045] In the description of the present application, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the feature. In the description of the present application, "plurality" means two or more, unless otherwise clearly and specifically defined.

[0046] The weight of the relevant components mentioned in the specification of the examples of this application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the specification of the examples of this application, it is within the scope disclosed in the specification of the examples of this application. Specifically, the weight described in the specification of the examples of this application can be mass units known in the chemical industry such as μg, mg, g, and kg.

[0047] An embodiment of the present application provides a method for preparing a magnesium-zirconium master alloy, comprising steps S10 to S30:

[0048] Step S10: Melting metal magnesium under high-frequency induction conditions to obtain a first melt.

[0049] In some of the examples, in step S10 , the frequency of the high-frequency induction is 1000 Hz to 4000 Hz.

[0050] It can be understood that the frequency of high-frequency induction includes but is not limited to 1000HZ, 1100HZ, 1200HZ, 1500HZ, 1800HZ, 2000HZ, 2200HZ, 2500HZ, 2800HZ, 3000HZ, 3200HZ, 3500HZ, 3800HZ, and 4000HZ.

[0051] In some of the examples, in step S10, smelting is performed at a first temperature, which is 700°C to 800°C.

[0052] It can be understood that the first temperature includes but is not limited to 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 780°C, and 800°C.

[0053] In some of the examples, in step S10, the temperature of the first melt is 680°C to 780°C.

[0054] It can be understood that the temperature of the first melt includes but is not limited to 680°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, and 780°C.

[0055] In some of the examples, in step S10 , the purity of magnesium is ≥ 99.95%.

[0056] Step S20: adding metal zirconium to the first melt, and performing alternating stirring under low-frequency induction conditions to obtain a second melt; the alternating stirring includes first stirring, second stirring and third stirring; the direction of the first stirring is that the upper melt flows upward from the center and flows downward from the side walls, and the lower melt flows upward from the side walls and flows downward from the center; the direction of the second stirring is that the melt flows upward from the side walls and flows downward from the center; the direction of the third stirring is that the melt flows upward from the center and flows downward from the side walls.

[0057] Understandably, see Figure 1In the first stirring, the melt in the molten pool is divided into an upper melt and a lower melt. The flow directions of the upper melt and the lower melt are different. The upper melt flows upward from the center and downward from the side wall, while the lower melt flows upward from the side wall and downward from the center. This is conventional induction stirring; see Figure 2 In the second stirring, the melt is a whole, the melt flows upward from the side wall and downward from the center, which is reverse stirring; see Figure 3 In the third stirring, the melt is a whole, and the melt flows upward from the center and downward from the side wall, which is positive stirring. It can be further understood that the stirring directions of the first stirring, the second stirring and the third stirring are controlled by the induction circuit of the induction furnace itself.

[0058] In some of the examples, in step S20, the alternating stirring includes sequentially performing the third stirring and the second stirring, and then cyclically performing the first stirring, the second stirring, and the third stirring.

[0059] Furthermore, after the third stirring is performed for 5 to 90 minutes and the second stirring is performed for 5 to 30 minutes in sequence, the first stirring, the second stirring and the third stirring are repeated in a cycle.

[0060] In some of the examples, in step S20, the alternating stirring includes first performing the second stirring, and then cyclically performing the first stirring, the second stirring, and the third stirring.

[0061] Furthermore, the second stirring is performed for 5 to 90 minutes, and then the first stirring, the second stirring and the third stirring are performed in a cycle.

[0062] In some of the examples, in step S20, the alternating stirring includes first performing the third stirring, and then cyclically performing the first stirring, the second stirring, and the third stirring.

[0063] Furthermore, the third stirring is performed for 5 to 90 minutes, and then the first stirring, the second stirring and the third stirring are performed in a cycle.

[0064] In some examples, in step S20, the alternating stirring includes cyclically performing first stirring, second stirring, and third stirring.

[0065] It can be understood that the cycle of performing the first stirring, the second stirring and the third stirring means that after performing the first stirring, the second stirring and the third stirring in sequence, this is one cycle, and then performing the first stirring, the second stirring and the third stirring in sequence again, this is the second cycle.

[0066] In some of the examples, in step S20, the total time of alternating stirring is 0.5 h to 3 h.

[0067] It will be appreciated that the total time for alternating stirring includes, but is not limited to, 0.5 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.5 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.5 h, 2.8 h, and 3 h.

[0068] In some of the examples, in step S20, when the first stirring, the second stirring and the third stirring are cyclically performed, each stirring mode is independently maintained for 2 minutes to 15 minutes.

[0069] It is understandable that after the first stirring for 2 minutes, the second stirring can be carried out for 5 minutes, and then the third stirring can be carried out for 10 minutes; and then the first stirring can be continued.

[0070] In some of the examples, in step S20, the number of cycles is 1 to 6 times.

[0071] In some examples, in step S20, the frequency of the low-frequency sensing is 20 Hz to 200 Hz.

[0072] It can be understood that the frequencies of low-frequency induction include but are not limited to 20HZ, 50HZ, 70HZ, 80HZ, 100HZ, 120HZ, 140HZ, 150HZ, 160HZ, 180HZ, and 200HZ.

[0073] In some of the examples, in step S20, the alternating stirring is performed at a second temperature, and the second temperature is 700°C to 800°C.

[0074] It can be understood that the second temperature includes but is not limited to 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 780°C, and 800°C.

[0075] In some of the examples, in step S20, metal zirconium is immersed in the first melt through a feeding device.

[0076] In some of the examples, in step S20, before adding the metal zirconium into the first melt, the step further includes performing a depassivation treatment on the surface of the metal zirconium.

[0077] The ability of molten magnesium to dissolve zirconium is effectively enhanced by removing the surface passivation layer of metal zirconium.

[0078] In some of the examples, in step S20 , the purity of the metal zirconium is ≥ 99.4%.

[0079] In some examples, in step S20, the metal zirconium is selected from at least one of zirconium sponge and zirconium chips.

[0080] Furthermore, the particle size of the zirconium sponge is 0.5 mm to 15 mm, and the thickness of the zirconium chips is ≤1.2 mm.

[0081] In some examples, in step S20 , the metal zirconium accounts for 0.1 wt % to 40 wt % of the magnesium-zirconium master alloy.

[0082] It can be understood that the 0.1wt% to 40wt% of metallic zirconium in the magnesium-zirconium master alloy refers to the mass ratio of the zirconium element in the entire magnesium-zirconium master alloy; it can be further understood that the mass ratio of metallic zirconium in the magnesium-zirconium master alloy includes but is not limited to 0.1wt%, 0.5wt%, 1wt%, 2wt%, 5wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt%, 20wt%, 22wt%, 25wt%, 28wt%, 30wt%, 32wt%, 35wt%, 38wt%, and 40wt%.

[0083] Step S30: Under the action of the third stirring, the second melt is cast at a fixed point to obtain a magnesium-zirconium master alloy.

[0084] It can be understood that the fixed-point casting directly casts the second melt in the smelting furnace into the mold without transferring the second melt and then casting it into the mold; the fixed-point casting method effectively avoids the sedimentation of zirconium particles during the melt transfer process.

[0085] In some of the examples, in step S30, the fixed-point casting is performed at a third temperature, and the third temperature is 720°C to 780°C.

[0086] It can be understood that the third temperature includes but is not limited to 720°C, 730°C, 740°C, 750°C, 760°C, and 780°C.

[0087] In some of the examples, in step S30 , casting is performed under low frequency induction conditions.

[0088] Furthermore, casting is carried out from a discharge port on the side of the induction furnace, and a hydraulic cylinder is used to drive the furnace body to tilt, so as to maintain the position of the pouring port basically unchanged.

[0089] In some of the examples, in step S30, the height difference between the pouring gate and the mold is maintained at 30 mm to 80 mm.

[0090] In some of the examples, in step S30, the casting mold may be in the shape of a waffle ingot, a plate, or a block.

[0091] In some of the examples, the step of preparing the magnesium-zirconium master alloy is carried out in a three-phase induction atmosphere furnace, using a mixed atmosphere of SF6 and CO2 for protection, and the melting power of the three-phase induction atmosphere furnace is 20kW to 300kW.

[0092] It will be appreciated that the smelting power includes but is not limited to 20 kW, 50 kW, 80 kW, 100 kW, 150 kW, 180 kW, 200 kW, 220 kW, 250 kW, and 300 kW.

[0093] The preparation method of the magnesium-zirconium master alloy is to melt the metal magnesium under high-frequency induction conditions, then add the metal zirconium and stir alternately in different directions under low-frequency induction conditions. The low-frequency induction method with adjustable phase difference ensures that the stirring force strength and the melt flow direction are controllable, so that the zirconium particles in the cast magnesium-zirconium master alloy are fine, the zirconium particles are dispersed, the zirconium content is high, the component segregation is small, and the inclusions are less. The preparation process is simple, and compared with the traditional magnesium reduction method, the pollution to the environment is less.

[0094] An embodiment of the present application provides a magnesium-zirconium master alloy, which is prepared by the above-mentioned method for preparing the magnesium-zirconium master alloy.

[0095] One embodiment of the present application provides the use of the above-mentioned magnesium-zirconium master alloy in the preparation of magnesium-zirconium alloy products. Another embodiment of the present application provides a magnesium-zirconium alloy product, the material of which includes the above-mentioned magnesium-zirconium master alloy.

[0096] In some embodiments, the material of the magnesium-zirconium alloy product may be the above-mentioned magnesium-zirconium master alloy, that is, the magnesium-zirconium alloy product is directly prepared using the above-mentioned magnesium-zirconium master alloy. In other embodiments, the material of the magnesium-zirconium alloy product may include other materials in addition to the above-mentioned magnesium-zirconium master alloy. Specific embodiments

[0098] The following examples are given according to the magnesium-zirconium master alloy and the preparation method thereof of the present application. It can be understood that the magnesium-zirconium master alloy and the preparation method thereof of the present application are not limited to the following examples.

[0099] In the following embodiments and comparative examples, A stirring is the first stirring, in which the upper melt flows upward from the center and downward from the side walls, and the lower melt flows upward from the side walls and downward from the center; B stirring is the second stirring, in which the melt flows upward from the side walls and downward from the center; C stirring is the third stirring, in which the melt flows upward from the center and downward from the side walls.

[0100] Example 1

[0101] The materials are prepared according to the mass ratio of magnesium to sponge zirconium of 1:0.22 for a single furnace of 50kg. The metal magnesium is placed in a sealed three-phase induction atmosphere furnace and heated in a mixed atmosphere of 99% CO2 and 1% SF6 by high-frequency induction mode (90-100kW, 1400-1500HZ). After the magnesium is completely melted, zirconium is added. When zirconium is added, the temperature of the magnesium melt is between 740°C and 750°C. The induction furnace is adjusted to low frequency operation and divided into three stirring modes. The first stage is in C stirring mode (65-80kW, 80-120HZ), and the melting temperature is maintained at 740℃-750℃ for 40min; then the second stage is in B stirring mode (40-65kW, 40-80HZ), and the melting temperature is maintained at 730℃-750℃ for 5min; the third stage is coordinated stirring, and A stirring (40-50kW, 70-100HZ), B stirring (40-65kW, 40-80HZ), and C stirring (65-80kW, 80-120HZ) are carried out in turn. Each stage is operated for 3min in turn, and the cycle is repeated 3 times. Fixed-point casting is carried out from the side pouring port of the induction furnace. During the casting process, the induction furnace maintains low-frequency C stirring (70-80kW, 100-120HZ). The casting temperature is between 730℃ and 740℃. A cast iron mold is used to obtain a magnesium-zirconium alloy ingot. The overall photo is as follows Figure 4 As shown, the cross-sectional photograph is shown in Figure 5 The 100x microstructure diagram is shown in Figure 6, and the 500x microstructure diagram is shown in Figure 7.

[0102] Example 2

[0103] It is basically the same as Example 1, and the only difference is that after the induction furnace is adjusted to the low-frequency operation step, the three-stage stirring mode in Example 1 is replaced by a two-stage stirring mode, specifically: the induction furnace is adjusted to low-frequency operation, and the stirring mode is divided into two stages. The first stage is in the B stirring mode (40-65kW, 40-80HZ), and the smelting temperature is maintained at 740℃~750℃ for 45min; then the second stage is coordinated stirring, and A stirring (40-50kW, 70-100HZ), B stirring (40-65kW, 40-80HZ), and C stirring (65-80kW, 80-120HZ) are carried out in turn. Each stage is operated for 3min in turn, and the overall stirring time is the same as that in Example 1.

[0104] Example 3

[0105] It is basically the same as Example 1, and the only difference is that after the induction furnace is adjusted to the low-frequency operation step, the three-stage stirring mode in Example 1 is replaced by a two-stage stirring mode, specifically: the induction furnace is adjusted to low-frequency operation, and the stirring mode is divided into two stages. The first stage is in C stirring mode (65-80kW, 80-120HZ), and the smelting temperature is maintained at 740℃~750℃ for 45min; then the second stage is coordinated stirring, and A stirring (40-50kW, 70-100HZ), B stirring (40-65kW, 40-80HZ), and C stirring (65-80kW, 80-120HZ) are carried out in turn. The coordinated stirring of each stage is carried out for 3min in sequence, and the overall stirring time is the same as that in Example 1.

[0106] Example 4

[0107] It is basically the same as Example 1, the only difference is that after the induction furnace is adjusted to the low-frequency operation step, the three-stage stirring method in Example 1 is replaced by a collaborative stirring method, specifically: after the induction furnace is adjusted to the low-frequency operation, A stirring (40-50kW, 70-100HZ), B stirring (40-65kW, 40-80HZ), and C stirring (65-80kW, 80-120HZ) are carried out in sequence, and each stage is operated for 10 minutes in sequence. The overall stirring time is the same as that in Example 1.

[0108] Comparative Example 1

[0109] Comparative Example 1 is a Mg-30Zr master alloy commercially available from Ganzhou Feiteng Light Alloy Co., Ltd., which is prepared by magnesium thermal reduction method. The ingot is a waffle ingot. The overall photo is as follows: Figure 8 As shown, the cross-sectional photograph is shown in Fig. 9 The 100x microstructure diagram is shown in FIG10 , and the 500x microstructure diagram is shown in FIG11 .

[0110] Comparative Example 2

[0111] The materials are prepared according to the mass ratio of 50kg per furnace and magnesium to sponge zirconium of 1:0.22. The metal magnesium is placed in a traditional medium frequency induction atmosphere furnace for smelting. The smelting is carried out under medium frequency induction conditions (30-40kW, 800-1000HZ). After the metal magnesium is completely melted, zirconium is added and A stirring is continued under medium frequency induction conditions. The overall stirring time is the same as that in Example 1. Fixed-point casting is carried out from the side pouring port of the induction furnace. During the casting process, the induction furnace maintains medium frequency A stirring operation. The casting temperature is between 730℃ and 740℃. A cast iron mold is used to obtain a magnesium-zirconium alloy ingot. The overall photo of the ingot is shown in the figure. Fig.12 As shown, the cross-sectional photograph is shown in Fig.13 14 shows the microstructure diagram at 100 times magnification, and 15 shows the microstructure diagram at 500 times magnification.

[0112] from Figures 4 to 15 It can be seen that, compared with the comparative example, the magnesium-zirconium master alloy obtained by the preparation method in the embodiment has a bright and smooth ingot appearance, few fracture inclusions, and zirconium particles are evenly distributed along the magnesium matrix in the microstructure.

[0113] Comparative Example 3

[0114] It is basically the same as Example 1, except that after the induction furnace is adjusted to low-frequency operation, only A stirring (40-50kW, 70-100HZ) is performed, and the overall stirring time is the same as that of Example 1.

[0115] Comparative Example 4

[0116] It is basically the same as Example 1, except that Comparative Example 4 adopts a conventional casting method, that is, the melt is first poured into a transfer bag and then cast into a mold.

[0117] Comparative Example 5

[0118] It is basically the same as Example 1, except that, in the step of fixed-point casting from the side pouring port of the induction furnace in Example 5, the induction furnace maintains low-frequency A stirring (40-50kW, 70-100HZ) during the casting process, and the casting temperature is between 730℃ and 740℃.

[0119] Comparative Example 6

[0120] It is basically the same as Example 1, except that, in the step of fixed-point casting from the side pouring port of the induction furnace in Example 6, the induction furnace maintains low-frequency B stirring (40-65kW, 40-80HZ) during the casting process, and the casting temperature is between 730℃ and 740℃.

[0121] The zirconium contents of different magnesium-zirconium alloy ingots from the same heat obtained in each embodiment and comparative example were tested, and the results are shown in Table 1.

[0122] Table 1 Zirconium content of different magnesium-zirconium alloy ingots from the same batch

[0123] Test (wt%) 1# Ingot 2# Ingot 3# Ingot 4# Ingot 5# Ingot Example 1 19.91 19.85 20.13 20.44 20.37 Example 2 18.61 18.56 19.25 20.54 21.90 Example 3 19.23 19.29 19.78 20.18 20.54 Example 4 18.57 18.20 18.61 19.22 19.39 Comparative Example 2 13.47 14.79 16.22 17.57 23.60 Comparative Example 3 15.56 16.23 17.43 22.22 22.84 Comparative Example 4 17.45 18.16 20.52 21.06 22.84 Comparative Example 5 16.83 17.38 18.20 19.31 21.78 Comparative Example 6 15.02 15.28 17.43 17.85 22.68

[0124] It can be seen from Table 1 that when the same proportion of metallic zirconium is added, the zirconium element yield in the magnesium-zirconium alloy ingots prepared in the embodiment is higher than that in the comparative example, especially in Example 1, the zirconium content is close to the designed 20wt% zirconium content; and the zirconium content between different magnesium-zirconium alloy ingots in the same furnace is relatively small.

[0125] The zirconium content at different positions of the same magnesium-zirconium alloy ingot obtained in each embodiment and comparative examples 1 and 4 was tested, and the results are shown in Table 2.

[0126] Table 2 Zirconium content in different parts of the same magnesium-zirconium alloy ingot

[0127]

[0128]

[0129] It can be seen from Table 2 that, compared with Comparative Examples 1 and 4, the gravity segregation of the same magnesium-zirconium alloy ingot prepared in the embodiment is smaller in the upper, middle and lower parts.

[0130] The sizes of zirconium particles in the magnesium-zirconium alloy ingots of Example 1 and Comparative Example 1 were statistically analyzed. The size statistics of Example 1 and Comparative Example 1 are shown in FIG. Figure 16-17 shown.

[0131] from Figure 16-17 It can be seen that compared with Comparative Example 1, the size of the zirconium particles in the magnesium-zirconium alloy ingot prepared in Example 1 is smaller, indicating that the zirconium particle size is fine.

[0132] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0133] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the contents of the attached claims, and the description and drawings can be used to explain the contents of the claims.

Claims

1. A method for preparing a magnesium-zirconium master alloy, characterized in that: The following steps are involved: Melting metal magnesium under high-frequency induction conditions to obtain a first melt; Adding metal zirconium to the first melt, and performing alternating stirring under low-frequency induction conditions to obtain a second melt; the alternating stirring consists of a first stirring, a second stirring, and a third stirring; the first stirring direction is that the upper melt flows upward from the center and downward from the side walls, and the lower melt flows upward from the side walls and downward from the center; the second stirring direction is that the melt flows upward from the side walls and downward from the center; the third stirring direction is that the melt flows upward from the center and downward from the side walls; Under the action of the third stirring, the second melt is cast at a fixed point to obtain a magnesium-zirconium master alloy; The frequency of the high-frequency induction is 1000 HZ~4000 HZ, and the frequency of the low-frequency induction is 20 HZ~200 HZ.

2. The method for preparing a magnesium-zirconium master alloy according to claim 1, characterized in that: The alternating stirring is selected from one of the following (1) to (4): (1) After the third stirring and the second stirring are performed in sequence, the first stirring, the second stirring and the third stirring are performed in a cycle; (2) After the second stirring is performed, the first stirring, the second stirring and the third stirring are performed in a cycle; (3) After the third stirring is performed, the first stirring, the second stirring and the third stirring are performed in a cycle; (4) The first stirring, the second stirring and the third stirring are repeated in a cycle.

3. The method for preparing a magnesium-zirconium master alloy according to claim 2, characterized in that: The total time of the alternating stirring is 0.5 h to 3 h.

4. The method for preparing a magnesium-zirconium master alloy according to claim 1, characterized in that: The smelting is performed at a first temperature, and the alternating stirring is performed at a second temperature. The first temperature and the second temperature are independently 700° C. to 800° C.

5. The method for preparing a magnesium-zirconium master alloy according to claim 1, characterized in that: The fixed-point casting is performed at a third temperature, and the third temperature is 720°C to 780°C.

6. The method for preparing a magnesium-zirconium master alloy according to any one of claims 1 to 5, characterized in that: The step of preparing the magnesium-zirconium master alloy is carried out in a three-phase induction atmosphere furnace, using a mixed atmosphere of SF6 and CO2 for protection, and the melting power of the three-phase induction atmosphere furnace is 20 kW to 300 kW.

7. The method for preparing a magnesium-zirconium master alloy according to any one of claims 1 to 5, characterized in that: Before the step of adding metal zirconium into the first melt, the method further includes the step of performing a depassivation treatment on the surface of the metal zirconium.

8. The method for preparing a magnesium-zirconium master alloy according to any one of claims 1 to 5, characterized in that: The metal zirconium accounts for 0.1 wt% to 40 wt% of the magnesium-zirconium master alloy.

9. A magnesium-zirconium master alloy, characterized in that: The magnesium-zirconium intermediate alloy is prepared by the preparation method of any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for heating molten metal in tundish

    JP2000015403A

  • Electromagnetic agitation method for continuous casting of metal products having an elongate section

    US20070074845A1