Preparation method of iron-nitrogen-carbon sulfur-doped catalyst
By forming an iron-nitrogen-carbon sulfur-doped catalyst with an Fe-S2/N4 structure on carbon black, the problem of high overpotential in the oxygen reduction reaction of the air cathode in Zn-air batteries was solved, and the high-efficiency oxygen reduction performance of the catalyst was improved.
Patent Information
- Application Number
- CN202310048047.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-01-31
AI Technical Summary
The existing Zn-air battery exhibits high overpotential during the oxygen reduction reaction at the air cathode, resulting in low charge-discharge efficiency. Therefore, it is necessary to develop efficient and stable electrocatalysts.
Using carbon black as a support, an iron-nitrogen-carbon sulfur-doped catalyst with an Fe-S2/N4 structure is formed on it through a pyrolysis process. Using phenanthroline as a ligand, sulfur atoms are introduced to coordinate with iron ions to form efficient FeSNx sites, thereby improving catalytic performance.
It significantly improved the oxygen reduction activity of the catalyst, reduced the overpotential of the oxygen reduction reaction, and improved the charge and discharge efficiency of the Zn-air battery.
Smart Images

Figure CN116130678B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the preparation of electrocatalysts and is applied to the field of green energy storage devices, represented by rechargeable metal-based batteries. Background Technology
[0002] Over the past few decades, numerous efforts have been made to develop sustainable green energy systems, such as fuel cells, electrochemical water splitting systems, and metal-air batteries. Compared to widely used commercial lithium-ion batteries, metal-air batteries can obtain the required oxygen directly from the air. Furthermore, rechargeable Zn-air batteries have been extensively studied due to their high theoretical energy density, non-toxicity, low cost, and safety.
[0003] However, due to the slow oxygen kinetics during the multi-step electron transfer process at the air cathode, a large overpotential exists at the air cathode during charge-discharge cycles, severely hindering the practical application of ZABs. To address these limitations of ZABs, there is an urgent need to develop low-cost, high-efficiency electrocatalysts with long-term cycling stability. Carbon black, as a widely used activated carbon material, is not only inexpensive but also possesses a structure composed of fragmented graphite layers with numerous pores and abundant surface groups, facilitating surface modification with various chemical reagents. After treatment with numerous active sites, this structure ensures that carbon black will not collapse due to pyrolysis and catalytic reactions, while also endowing it with excellent adsorption properties. Nitrogen-containing heterocycles containing iron ions can fill the spaces between the fragmented graphite layers of carbon black. After pyrolysis, the nitrogen-containing heterocycles combine with the graphite layers to form iron-nitrogen (FeNx) sites, yielding an ORR catalyst. Since divalent iron is six-coordinated, this invention attempts to add non-metallic atoms around the iron atoms, replacing some of the nitrogen atoms in the six-coordinated configuration with iron with sulfur atoms to form FeSNx, thereby improving its catalytic performance. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a method for preparing a single-atom iron-nitrogen-carbon sulfur-doped catalyst using the coordination principle, comprising the following steps: The first step is the preparation of a solution of dithiophene or dibenzothiophene, phenanthroline, carbon black, and FeSO4·7H2O: A certain amount of dithiophene or dibenzothiophene is dissolved in N,N-dimethylformamide and a uniform dispersion is obtained under magnetic stirring. phenanthroline, carbon black, and FeSO4·7H2O are then dispersed in methanol and stirred uniformly under magnetic stirring. The purpose of this step is to ensure uniform dispersion of the solution, facilitating mixing in subsequent steps.
[0005] The second step is the preparation of the FeSNC solution: the solution of dithiophene or dibenzothiophene is added dropwise to the solution of phenanthroline, and a uniform dispersion is obtained under magnetic stirring; the solution of FeSO4·7H2O is added dropwise to the dispersion of carbon black, and the mixture is stirred evenly under magnetic stirring; the two solutions are mixed again and stirred evenly under magnetic stirring.
[0006] The third step is the preparation of the FeSNC precursor: the excess solvent in the obtained FeSNC solution is evaporated at a certain temperature.
[0007] The fourth step is the preparation of the FeSNC catalyst: the obtained powdered FeSNC precursor is pyrolyzed under an argon atmosphere to obtain the catalyst. During the pyrolysis process, the nitrogen-containing heterocycles combine with the graphite layer to form iron-sulfur-nitrogen (FeSNx) sites with iron and sulfur.
[0008] In the second step, the molar ratio of FeSO4·7H2O, phenanthroline, dithiophene, or dibenzothiophene is 0.30~1.0 : 1.0 : 0.30~1.0, and the molar ratio of carbon black to FeSO4·7H2O is 100 : 1~2.
[0009] In the fourth step, the pyrolysis temperature is 700~900 ℃ and the time is 3-5 h.
[0010] The beneficial effects of this invention are as follows: The catalyst preparation method provided by this invention has the following characteristics. Using highly conductive and surface-active carbon black as a support, and phenanthroline with a strong coordination effect as a ligand, a transition metal single-atom iron is loaded. Simultaneously, sulfur atoms are introduced to further coordinate with iron ions, thereby adsorbing onto the carbon black surface to form a precursor structure resembling "(a) Fe-S2 / N4" as shown in the figure. Compared to the precursor structures "(b) Fe-N6" and "(c) Fe-N4" without the introduction of a sulfur source, the Fe-S2 / N4 precursor structure, after high-temperature sintering, yields a sulfur-doped iron-nitrogen-carbon material. Subsequent electrochemical tests of the material show that the incorporation of sulfur can further improve the catalytic oxygen reduction activity of the iron-nitrogen-carbon material.
[0011] . Attached Figure Description
[0012] Figure 1 a is the ORR diagram of the sample in Example 1, and b is the number of transferred electrons and the hydrogen peroxide yield of the sample in Example 1.
[0013] Figure 2 a is the ORR diagram of the sample in Example 2, and b is the number of transferred electrons and hydrogen peroxide yield of the sample in Example 2.
[0014] Figure 3a is the ORR diagram of the sample in Example 3, and b is the number of transferred electrons and hydrogen peroxide yield of the sample in Example 3.
[0015] Figure 4 a is the ORR diagram of the sample in Example 4, and b is the number of transferred electrons and hydrogen peroxide yield of the sample in Example 4.
[0016] Figure 5 a is the ORR diagram of the sample in Example 5, and b is the number of transferred electrons and hydrogen peroxide yield of the sample in Example 5.
[0017] Figure 6 a is the ORR diagram of the sample in Example 6, and b is the number of transferred electrons and hydrogen peroxide yield of the sample in Example 6.
[0018] Figure 7 a is the ORR diagram of the sample in Example 7, and b is the number of transferred electrons and hydrogen peroxide yield of the sample in Example 7.
[0019] Figure 8 a is the ORR diagram of the sample in Example 8, and b is the number of transferred electrons and hydrogen peroxide yield of the sample in Example 8.
[0020] Figure 9 The SEM images of Example 1, (a) have a magnification of 100,000 times; (b) have a magnification of 20,000 times.
[0021] Figure 10 The SEM images of Example 4, (a) have a magnification of 100,000 times; (b) have a magnification of 20,000 times.
[0022] Figure 11 The SEM images of Example 5, (a) have a magnification of 100,000 times; (b) have a magnification of 20,000 times.
[0023] Figure 12 EDS spectrum of Example 1.
[0024] Figure 13 EDS spectrum of Example 4.
[0025] Figure 14 EDS spectrum of Example 5. Detailed Implementation
[0026] Characterization conditions: The ORR test method in this embodiment of the invention is as follows: Take 980 μL of water, 980 μL of ethanol, and 40 μL of Nafion, mix them thoroughly, then take 10 mg of sample and add it to the solution. Sonicate for 2 h to disperse the sample evenly. Then, drop the resulting slurry onto a rotating ring electrode with a loading of 0.8 mg / cm². 2The test was then conducted using a three-electrode system consisting of a reference electrode (mercuric oxide), a counter electrode (carbon rod), and a working electrode in an oxygen-saturated 0.1 M KOH solution.
[0027] Example 1 120 mg of carbon black was dispersed in 8 mL of methanol, 56 mg of FeSO4·7H2O was dissolved in 1 mL of methanol, and 120 mg of phenanthroline was dissolved in 1 mL of methanol. The solutions were stirred evenly separately. Then, the FeSO4·7H2O solution and the phenanthroline solution were added dropwise to the carbon black dispersion and stirred evenly. The excess solvent in the uniformly dispersed solution was then evaporated at 60 °C. Stirring was then stopped, and the solution was further dried at 80 °C for 2 h. Finally, the obtained powdered FeSNC precursor was pyrolyzed at 800 °C for 3 h under an argon atmosphere.
[0028] Figure 1 a shows the ORR curve of the sample from Example 1, with an initial potential of -0.055 V vs RHE and a limiting current density of 5.53 mA / m². 2 The half-wave potential is 0.78 V vs RHE. Figure 1 b represents the number of transferred electrons and the yield of hydrogen peroxide byproduct in the sample of Example 1. It can be concluded that the number of transferred electrons is close to 4 and the yield of hydrogen peroxide is about 0.4%.
[0029] Figure 12 The image shows the EDS spectrum of Example 1, where the atomic percentage of C is 77.89% and the atomic percentage of Fe is 4.18%.
[0030] Example 2 120 mg of carbon black was dissolved in 8 mL of methanol, 56 mg of FeSO4·7H2O was dissolved in 1 mL of methanol, 120 mg of phenanthroline was dissolved in 1 mL of methanol, and 37 mg of dibenzothiophene was dissolved in 1 mL of N,N-dimethylformamide. The solutions were stirred thoroughly. Then, the dibenzothiophene solution was added dropwise to the phenanthroline solution, and the FeSO4·7H2O solution was added dropwise to the carbon black dispersion. The solutions were stirred thoroughly again, and then the mixed solutions were stirred thoroughly once more. The excess solvent in the uniformly dispersed solution was evaporated at 60 °C, and then stirring was stopped. The solution was further dried at 80 °C for 2 h. Finally, the obtained powdered FeSNC precursor was pyrolyzed at 800 °C for 3 h under an argon atmosphere.
[0031] Figure 2 a shows the ORR curve of the sample in Example 2, with an onset potential of -0.054 V vs RHE and a limiting current density of 5.04 mA / cm². 2The half-wave potential is 0.8 V vs RHE. Figure 2 b represents the number of transferred electrons and the yield of hydrogen peroxide byproduct in the sample of Example 2. It can be concluded that the number of transferred electrons is close to 4 and the yield of hydrogen peroxide is about 0.7%.
[0032] Example 3 120 mg of carbon black was dissolved in 8 mL of methanol, 56 mg of FeSO4·7H2O was dissolved in 1 mL of methanol, 120 mg of phenanthroline was dissolved in 1 mL of methanol, and 33.5 mg of dithiophene was dissolved in 1 mL of N,N-dimethylformamide. The solutions were stirred thoroughly. Then, the dithiophene solution was added dropwise to the phenanthroline solution, and the FeSO4·7H2O solution was added dropwise to the carbon black dispersion. The solutions were stirred thoroughly again, and then the uniformly dispersed solution was evaporated at 60 °C to remove excess solvent. Stirring was then stopped, and the solution was further dried at 80 °C for 2 h. Finally, the obtained powdered FeSNC precursor was pyrolyzed at 800 °C for 3 h under an argon atmosphere.
[0033] Figure 3 a shows the ORR curve for the sample in Example 3, with an initial potential of -0.064 V vs RHE and a limiting current density of 6.46 mA / cm². 2 The half-wave potential is 0.81 V vs RHE. Figure 3 b represents the number of transferred electrons and the yield of hydrogen peroxide byproduct in the sample of Example 3. It can be concluded that the number of transferred electrons is close to 4 and the yield of hydrogen peroxide is about 0.5%.
[0034] Example 4 120 mg of carbon black was dissolved in 8 mL of methanol, 28 mg of FeSO4·7H2O in 1 mL of methanol, 36.3 mg of phenanthroline in 1 mL of methanol, and 18.5 mg of dibenzothiophene in 1 mL of N,N-dimethylformamide. Each solution was stirred thoroughly. Then, the dibenzothiophene solution was added dropwise to the phenanthroline solution, and the FeSO4·7H2O solution was added dropwise to the carbon black dispersion. Each solution was stirred thoroughly again, and the two solutions were then mixed thoroughly once more. The excess solvent was evaporated at 60 °C, and stirring was stopped. The mixture was then further dried at 80 °C for 2 h. Finally, the obtained powdered FeSNC precursor was pyrolyzed at 800 °C for 3 h under an argon atmosphere.
[0035] Figure 4 a shows the ORR curve for sample 4, with an onset potential of -0.045 V vs RHE and a limiting current density of 4.56 mA / cm². 2The half-wave potential is 0.85 V vs RHE. Figure 4 b represents the number of transferred electrons and the yield of hydrogen peroxide byproduct in the sample of Example 4. It can be concluded that the number of transferred electrons is close to 4 and the yield of hydrogen peroxide is about 0.3%.
[0036] Figure 13 The image shows the EDS spectrum of Example 4, where the atomic percentage of C is 54.60%, the atomic percentage of S is 0.62%, and the atomic percentage of Fe is 2.04%.
[0037] Example 5 120 mg of carbon black was dissolved in 8 mL of methanol, 28 mg of FeSO4·7H2O was dissolved in 1 mL of methanol, 36.3 mg of phenanthroline was dissolved in 1 mL of methanol, and 16.74 mg of dithiophene was dissolved in 1 mL of N,N-dimethylformamide. The solutions were stirred thoroughly. Then, the dithiophene solution was added dropwise to the phenanthroline solution, and the FeSO4·7H2O solution was added dropwise to the carbon black dispersion. The solutions were stirred thoroughly again, and then the two solutions were mixed thoroughly. The excess solvent was evaporated at 60 °C, and stirring was stopped. The mixture was then further dried at 80 °C for 2 h. Finally, the obtained powdered FeSNC precursor was pyrolyzed at 800 °C for 3 h under an argon atmosphere.
[0038] Figure 5 a shows the ORR curve for the sample in Example 5, with an initial potential of -0.046 V vs RHE and a limiting current density of 4.56 mA / cm². 2 The half-wave potential is 0.89 V vs RHE. Figure 5 b represents the number of transferred electrons and the yield of hydrogen peroxide byproduct in the sample of Example 5. It can be concluded that the number of transferred electrons is close to 4 and the yield of hydrogen peroxide is about 0.5%.
[0039] Figure 14 The image shows the EDS spectrum of Example 5, where the atomic percentage of C is 73.45%, the atomic percentage of S is 3.54%, and the atomic percentage of Fe is 4.65%.
[0040] Example 6 120 mg of carbon black was dissolved in 8 mL of methanol, 28 mg of FeSO4·7H2O was dissolved in 1 mL of methanol, 36.3 mg of phenanthroline was dissolved in 1 mL of methanol, and 16.74 mg of dithiophene was dissolved in 1 mL of N,N-dimethylformamide. The solutions were stirred thoroughly. Then, the dithiophene solution was added dropwise to the phenanthroline solution, and the FeSO4·7H2O solution was added dropwise to the carbon black dispersion. The solutions were stirred thoroughly again, and then the two solutions were mixed thoroughly. The excess solvent was evaporated at 60 °C, and stirring was stopped. The mixture was then further dried at 80 °C for 2 h. Finally, the obtained powdered FeSNC precursor was pyrolyzed at 700 °C for 3 h under an argon atmosphere.
[0041] Figure 6 a shows the ORR curve for the sample in Example 6, with an initial potential of -0.05 V vs RHE and a limiting current density of 5.03 mA / cm². 2 The half-wave potential is 0.87 V vs RHE. Figure 6 b represents the number of transferred electrons and the yield of hydrogen peroxide byproduct in the sample of Example 6. It can be concluded that the number of transferred electrons is close to 4 and the yield of hydrogen peroxide is about 0.2%.
[0042] Example 7 120 mg of carbon black was dissolved in 8 mL of methanol, 28 mg of FeSO4·7H2O was dissolved in 1 mL of methanol, 36.3 mg of phenanthroline was dissolved in 1 mL of methanol, and 16.74 mg of dithiophene was dissolved in 1 mL of N,N-dimethylformamide. The solutions were stirred thoroughly. Then, the dithiophene solution was added dropwise to the phenanthroline solution, and the FeSO4·7H2O solution was added dropwise to the carbon black dispersion. The solutions were stirred thoroughly again, and then the two solutions were mixed thoroughly. The excess solvent was evaporated at 60 °C, and stirring was stopped. The mixture was then further dried at 80 °C for 2 h. Finally, the obtained powdered FeSNC precursor was pyrolyzed at 750 °C for 3 h under an argon atmosphere.
[0043] Figure 7 a shows the ORR curve for sample 7 of Example 7, with an initial potential of -0.05 V vs RHE and a limiting current density of 5.03 mA / cm². 2 The half-wave potential is 0.84 V vs RHE. Figure 7 b represents the number of transferred electrons and the yield of hydrogen peroxide byproduct in the sample of Example 7. It can be concluded that the number of transferred electrons is close to 4 and the yield of hydrogen peroxide is about 0.3%.
[0044] Example 8 120 mg of carbon black was dissolved in 8 mL of methanol, 28 mg of FeSO4·7H2O was dissolved in 1 mL of methanol, 36.3 mg of phenanthroline was dissolved in 1 mL of methanol, and 16.74 mg of dithiophene was dissolved in 1 mL of N,N-dimethylformamide. The solutions were stirred thoroughly. Then, the dithiophene solution was added dropwise to the phenanthroline solution, and the FeSO4·7H2O solution was added dropwise to the carbon black dispersion. The solutions were stirred thoroughly, and then the two mixtures were thoroughly combined. The excess solvent was evaporated at 60 °C, and stirring was stopped. The mixture was then further dried at 80 °C for 2 h. Finally, the obtained powdered FeSNC precursor was pyrolyzed at 900 °C for 3 h under an argon atmosphere.
[0045] Figure 8 a shows the ORR curve for sample 8 of Example 8, with an initial potential of -0.05 V vs RHE and a limiting current density of 4.95 mA / cm². 2 The half-wave potential is 0.83 V vs RHE. Figure 8 b represents the number of transferred electrons and the yield of hydrogen peroxide byproduct in the sample of Example 8. It can be concluded that the number of transferred electrons is close to 4 and the yield of hydrogen peroxide is about 0.3%.
Claims
1. A method for preparing an iron-nitrogen-carbon sulfur-doped catalyst, characterized in that, Includes the following steps: Preparation of S1, dithiophene, phenanthroline, carbon black, and FeSO4·7H2O solution: A certain amount of dithiophene was dissolved in N,N-dimethylformamide and stirred evenly to obtain a dithiophene dispersion; phenanthroline, carbon black, and FeSO4·7H2O were dispersed in methanol and stirred evenly to obtain methanol solutions of phenanthroline, carbon black, and FeSO4·7H2O. Preparation of S2 and FeSNC solution: A dispersion of dithiophene is added dropwise to a methanol solution of phenanthroline and stirred until homogeneous; a methanol solution of FeSO4·7H2O is added dropwise to a methanol solution of carbon black and stirred until homogeneous; the two solutions are mixed again and stirred until homogeneous to obtain the FeSNC solution; the molar ratio of FeSO4·7H2O, phenanthroline, dithiophene, or dibenzothiophene is 0.30~1.0 : 1.0 : 0.30~1.0, and the molar ratio of carbon black to FeSO4·7H2O is 100 : 1~2; S3. Preparation of FeSNC precursor: The obtained FeSNC solution was evaporated to dryness to obtain powdered FeSNC precursor; S4. Preparation of FeSNC catalyst: The obtained powdered FeSNC precursor was pyrolyzed under an argon atmosphere at a temperature of 700~900 ℃ for 3-5 h to obtain the catalyst.
2. The preparation method according to claim 1, characterized in that, The aforementioned dithiophene is replaced with dibenzothiophene.
Citation Information
Patent Citations
Nitrogen and sulfur doped iron monatomic loaded porous carbon catalyst and preparation method thereof
CN115064704A