Catalyst and preparation method thereof and application in preparing 1,3-butanediol by hydrogenation of 3-hydroxybutyraldehyde

By using NiCo2O4-Al2O3 catalyst to hydrogenate in a fixed bed reactor, the problem of insufficient catalyst activity and selectivity in the prior art is solved, and efficient 1,3-butanediol production is achieved, which is suitable for large-scale industrial applications.

CN116139864BInactive Publication Date: 2024-11-19DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202111383067.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-22
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing 1,3-butanediol chemical synthesis process, the activity and selectivity of the catalyst are insufficient, making it difficult to achieve efficient large-scale production.

Method used

NiCo2O4-Al2O3 was used as a catalyst and prepared by high-temperature calcination method, and contacted with an aqueous solution of 3-hydroxybutyraldehyde in a fixed bed reactor, and hydrogenation reaction was carried out to produce 1,3-butylene glycol.

Benefits of technology

The conversion rate of 3-hydroxybutyraldehyde and the selectivity of 1,3-butylene glycol are improved, and the catalyst preparation method is stable and controllable, with a fast reaction speed, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003366323720000051
    Figure BDA0003366323720000051
  • Figure BDA0003366323720000061
    Figure BDA0003366323720000061
  • Figure BDA0003366323720000071
    Figure BDA0003366323720000071
Patent Text Reader

Abstract

The present application discloses a catalyst and its preparation method and the application in 3-hydroxybutyraldehyde hydrogenation to prepare 1,3-butanediol, the catalyst comprising an active component and a carrier; the active component is NiCo2O4, and the carrier is Al2O3. The present application also discloses a method for preparing the catalyst, the method comprising obtaining NiCo2O4 by a high temperature calcination method, and then mixing NiCo2O4 and Al2O3 by a mechanical mixing method or a wet mixing method to calcine to obtain the catalyst. The present application also discloses a method for preparing 1,3-butanediol by 3-hydroxybutyraldehyde hydrogenation reaction using the catalyst. The catalyst provided in the present application is applied to the reaction of preparing 1,3-butanediol by hydrogenation, and the catalyst has good activity, high 3-hydroxybutyraldehyde conversion rate and 1,3-butanediol selectivity, and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a catalyst and a preparation method thereof and application in the preparation of 1,3-butanediol by hydrogenation of 3-hydroxybutyraldehyde, belonging to the field of chemical industry. Background Art

[0002] 1,3-Butanediol can also be used to produce unsaturated polyester resins, plasticizers, humidifiers and softeners, etc., and has a wide range of applications in industrial production.

[0003] At present, there are two main methods for the synthesis of 1,3-butanediol: biological method and chemical synthesis method. Although the biological method has mild production conditions, high selectivity, and less waste emissions, the output is low and it is difficult to achieve large-scale production. The chemical synthesis method mainly includes methods such as condensation and hydrolysis of propylene and formaldehyde, hydrogenation and ring opening of 3-hydroxytetrahydrofuran, and condensation and hydrogenation of acetaldehyde. Among them, acetaldehyde condensation and hydrogenation is currently the most important chemical synthesis production process route, and the products of this process route account for more than 95% of the market share. In this process, it is mainly divided into two steps: condensation of acetaldehyde to generate 3-hydroxybutyraldehyde and hydrogenation of 3-hydroxybutyraldehyde to generate 1,3-butanediol. Among them, the preparation of hydrogenation catalysts and optimization of hydrogenation processes are one of the key contents of research.

[0004] Chinese application CN112452331A uses Ni / Mg5Al2O8 as a catalyst to carry out 3-hydroxybutyraldehyde hydrogenation to prepare 1,3-butanediol in a kettle reaction, with a reaction conversion rate of 100% and a selectivity of 99.5%. Chinese applications CN109422624A and CN109422635A disclose a method for preparing 1,3-butanediol by hydrogenating 3-hydroxybutyraldehyde in a fixed bed reactor, wherein the catalyst is a supported nickel catalyst; Chinese application CN111393259A uses 3-hydroxybutyraldehyde as a raw material, and carries out a catalytic hydrogenation reaction in a trickle bed reactor under the conditions of 20 to 100°C and 1.0 to 8.0 MPa of hydrogen atmosphere using a supported metal nickel catalyst and an alkaline solvent, wherein the hydrogenation conversion rate of 3-hydroxybutyraldehyde can reach 86%, and the selectivity of 1,3-butanediol can reach 88%; Chinese applications CN110668917A and CN210945432U carry out a hydrogenation reaction between 3-hydroxybutyraldehyde and hydrogen in a tower reactor, and the purity of the refined 1,3-butanediol is greater than 99.6% and has no odor. Summary of the invention

[0005] In one aspect of the present application, a catalyst is provided, which can be used in the hydrogenation reaction to prepare 1,3-butanediol and improve the conversion rate of 3-hydroxybutyraldehyde and the selectivity of 1,3-butanediol, and the catalyst component is NiCo2O4-Al2O3.

[0006] Optionally, the catalyst active component contains NiCo2O4; the carrier includes Al2O3;

[0007] Optionally, the active component accounts for 5 to 30 wt% of the catalyst;

[0008] Optionally, the upper limit of the active component content in the total catalyst is selected from 30wt% and 20wt%, and the lower limit is selected from 5wt% and 10wt%;

[0009] Optionally, the catalyst is used for the hydrogenation reaction to prepare 1,3-butanediol.

[0010] Another aspect of the present application provides a method for preparing the catalyst, the method comprising the following steps:

[0011] (1) NiCo2O4 is prepared by high temperature calcination method;

[0012] (2) The carrier is mixed with the NiCo2O4 obtained in step (1) and then calcined I to obtain the catalyst.

[0013] Optionally, the mixing method of NiCo2O4 and the carrier Al2O3 is selected from any one of a mechanical mixing method and a wet mixing method.

[0014] Optionally, the specific steps of the high temperature calcination method include:

[0015] The nickel source, cobalt source and solvent are ground and mixed in a mortar, dried, and calcined II to obtain NiCo2O4.

[0016] Optionally, the nickel source is selected from at least one of nickel nitrate, nickel sulfate and nickel acetate;

[0017] Optionally, the cobalt source is selected from at least one of cobalt nitrate, cobalt sulfate and cobalt acetate.

[0018] Optionally, in the nickel source and the cobalt source, the molar ratio of Ni element to Co element is (0.9-1):2;

[0019] Optionally, the upper limit of the molar ratio of the Ni element to the Co element can be independently selected from 0.95:2 and 1:2, and the lower limit is 0.9:2 and 0.95:2.

[0020] Optionally, the solvent is selected from one of water, ethanol, and a mixed solution of ethanol and water.

[0021] Optionally, in the mixed solution of ethanol and water, the mass ratio of ethanol to water is 1:1.

[0022] Optionally, the solvent is deionized water.

[0023] Optionally, the volume ratio of the total solid mass of the nickel source and the cobalt source to the solvent is 1: (6-7) g / ml.

[0024] Optionally, the upper limit of the volume ratio of the total solid mass of the nickel source and the cobalt source to the solvent can be independently selected from 1:6 g / ml, 1:6.5 g / ml, and the lower limit can be independently selected from 1:7 g / ml, 1:6.5 g / ml.

[0025] Optionally, the calcination II temperature is 800° C. to 1200° C., and the calcination II time is 12 h to 24 h.

[0026] Optionally, the upper limit of the calcination II temperature can be independently selected from 1200°C, 1100°C, 1000°C, 900°C, and the lower limit can be independently selected from 800°C, 900°C, 1000°C, 1100°C; the upper limit of the calcination II time can be independently selected from 24h, 20h, 16h, and the lower limit can be independently selected from 12h, 16h, 20h.

[0027] As a specific implementation, the specific steps of preparing the mixture by the high temperature calcination method include:

[0028] The nickel source, the cobalt source and the solvent are mixed, ground in a mortar for a period of time to fully mix the nickel source and the cobalt source, and dried to obtain a mixture;

[0029] Optionally, the grinding time using a mortar is 30 to 60 minutes;

[0030] Optionally, the upper limit of the time for grinding in a mortar can be independently selected from 60 minutes, 50 minutes, and 40 minutes, and the lower limit can be independently selected from 30 minutes, 40 minutes, and 50 minutes;

[0031] Optionally, the drying temperature is 100° C. to 120° C., and the drying time is 8 h to 12 h.

[0032] Optionally, the upper limit of the drying temperature can be independently selected from 120°C and 110°C, and the lower limit can be independently selected from 100°C and 110°C; the upper limit of the drying time can be independently selected from 12h and 10h, and the lower limit can be independently selected from 8h and 10h.

[0033] Optionally, the calcination temperature I is 500° C. to 600° C., and the calcination time I is 2 h to 6 h.

[0034] Optionally, the upper limit of the calcination temperature I may be independently selected from 600°C and 550°C, and the lower limit may be independently selected from 500°C and 550°C.

[0035] Optionally, the upper limit of the calcination time I can be independently selected from 6h, 5h, 4h, 3h, and the lower limit can be independently selected from 2h, 3h, 4h, 5h.

[0036] In another aspect of the present application, a method for preparing 1,3-butanediol by hydrogenating 3-hydroxybutyraldehyde is provided, wherein H2 and an aqueous solution containing 3-hydroxybutyraldehyde are contacted with a catalyst to react to obtain a product containing 1,3-butanediol;

[0037] The catalyst comprises at least one of the above catalysts or at least one of the catalysts prepared by the above method.

[0038] Optionally, the reaction is carried out using a fixed bed reactor.

[0039] Optionally, the catalyst is loaded in a fixed bed reactor.

[0040] Optionally, the mass fraction of the aqueous solution containing 3-hydroxybutyraldehyde is 20 to 50%;

[0041] Optionally, the upper limit of the mass fraction of the 3-hydroxybutyraldehyde aqueous solution can be independently selected from 50%, 40%, and 30%, and the lower limit can be independently selected from 20%, 30%, and 40%.

[0042] Optionally, the reaction temperature of the contact reaction is 70° C. to 110° C., the reaction time is 1 h to 4 h, and the reaction pressure is 2 to 5 MPa.

[0043] Optionally, the upper limit of the reaction temperature may be independently selected from 110°C, 100°C, 90°C, 80°C, and the lower limit of the reaction temperature may be independently selected from 70°C, 80°C, 90°C, 100°C.

[0044] Optionally, the upper limit of the reaction time can be independently selected from 4h, 3h, and 2h, and the lower limit of the reaction time can be independently selected from 1h, 2h, and 3h;

[0045] Optionally, the upper limit of the reaction pressure can be independently selected from 5Mpa, 4Mpa, and 3Mpa, and the lower limit of the reaction pressure can be independently selected from 2Mpa, 3Mpa, and 4Mpa.

[0046] Optionally, the mass space velocity of the aqueous solution containing 3-hydroxybutyraldehyde is 2h -1 ~4h -1 ;

[0047] Optionally, the upper limit of the mass space velocity of the aqueous solution containing 3-hydroxybutyraldehyde can be independently selected from 4h -1 , 3h -1 , the lower limit can be independently selected from 2h -1 , 3h -1 .

[0048] Optionally, the mass space velocity of H2 is 80h -1 ~120h -1 .

[0049] Optionally, the upper limit of the mass space velocity of H2 is selected from 120h -1 , 110h -1 、100h -1 , 90h -1 , the lower limit is selected from 80h -1 , 90h -1 、100h -1 , 110h -1 .

[0050] As a specific embodiment, the method for preparing 1,3-butanediol by hydrogenating 3-hydroxybutyraldehyde comprises the following steps:

[0051] The catalyst is loaded in a fixed bed reactor; H2 and raw materials are introduced, and the raw materials are contacted with the catalyst in the reactor and reacted for 1h to 4h at a temperature of 70°C to 110°C, and the reaction pressure is 2 to 5Mpa to obtain a product containing 1,3-butanediol;

[0052] The raw material is a mixed solution of 3-hydroxybutyraldehyde and deionized water.

[0053] The beneficial effects of this application include:

[0054] 1) The catalyst provided in the present application can be applied to the reaction of hydrogenating 3-hydroxybutyraldehyde to prepare 1,3-butanediol, and improve the conversion rate of acetaldehyde and the selectivity of the generated 3-hydroxybutyraldehyde.

[0055] 2) The preparation method of the catalyst provided in this application is stable, controllable and reproducible.

[0056] 3) The method for preparing 1,3-butanediol by hydrogenation of 3-hydroxybutyraldehyde provided in the present application uses the catalyst provided in the present application, has a fast reaction speed and a high yield, and can be applied to large-scale production.

[0057] 4) The catalyst provided in the present application is used in the hydrogenation reaction to prepare 1,3-butanediol. The catalyst has good activity, high 3-hydroxybutyraldehyde conversion rate and 1,3-butanediol selectivity, and good stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 Catalyst 1 # X-ray powder diffraction pattern of NiCo2O4 DETAILED DESCRIPTION

[0059] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0060] Unless otherwise specified, the raw materials and catalysts in the examples of the present application were purchased from commercial sources. The gas chromatograph was a 7890B gas chromatograph from Agilent.

[0061] The conversion rate and selectivity calculation formula in the examples of the present application are as follows (with 3-hydroxybutyraldehyde conversion rate as the evaluation index):

[0062] 3-Hydroxybutyraldehyde conversion rate = (initial carbon number of 3-hydroxybutyraldehyde - carbon number of 3-hydroxybutyraldehyde in the product) * 100 / initial molar number of 3-hydroxybutyraldehyde

[0063] 1,3-Butanediol selectivity = carbon number of 1,3-butanediol*100 / ∑(carbon number of 1,3-butanediol+carbon number of other products)

[0064] Example 1 Preparation of Catalyst

[0065] Taking No. 1 in Table 1 as an example, nickel nitrate and cobalt nitrate (Ni and Co molar ratio 1:2) were mixed in deionized water (solid-liquid ratio 1:6 g / ml) and ground in a mortar for 40 minutes. The mixture was placed in a 100°C oven for 12 hours to obtain a mixture; the mixture was then placed in a high-temperature furnace and calcined at 1200°C for II20 hours to obtain NiCo2O4. NiCo2O4 was mixed with carrier Al2O3 by wet mixing (the active component accounted for 20wt% of the total catalyst content), and calcined at 550°C for I3h, which was recorded as catalyst 1. # .

[0066] According to the following steps, the types, amounts and reaction parameters of each raw material are adjusted to obtain a series of catalysts numbered 2 to 28, which are recorded as catalyst 2 # ~Catalyst 28 # , as shown in Table 1 below:

[0067] Table 1

[0068]

[0069]

[0070] The columns in Table 1 above are explained as follows:

[0071] Nickel source: nickel nitrate (Ni1), nickel sulfate (Ni2), nickel acetate (Ni3).

[0072] Cobalt sources: cobalt nitrate (Co1), cobalt sulfate (Co2), cobalt acetate (Co3).

[0073] Solvent: deionized water (solvent 1), ethanol (solvent 2), a mixed solution of ethanol and deionized water (mass ratio 1:1) (solvent 3).

[0074] Mixing methods of NiCo2O4 and carrier Al2O3: mechanical mixing method (method 1), wet mixing method (method 2).

[0075] in,

[0076] Mechanical mixing method: Grind NiCo2O4 and carrier Al2O3 in a mortar for 30 minutes or stir with a mechanical stirrer for 30 minutes;

[0077] Wet mixing method: Grind NiCo2O4, carrier Al2O3 and deionized water (solid-liquid ratio 1:7 g / ml) in a mortar for 30 minutes or place them in a beaker and stir with a magnetic stirrer for 30 minutes (rotation speed 300 rpm), and then dry them in an oven at 100°C.

[0078] Using Miniflex 600 X-ray diffractometer and Cu target, powder diffraction of NiCo2O4 of catalyst 1 was performed, and the diffraction peaks were consistent with the characteristic peaks of NiCo2O4 (such as Figure 1 shown).

[0079] Example 2

[0080] The catalyst is used for the hydrogenation reaction to produce 1,3-butanediol.

[0081] Catalyst 1 of sequence numbers 1 to 28 prepared in Example 1 # ~Catalyst 28 # , used for hydrogenation preparation of 1,3-butanediol, the catalyst is loaded in a fixed bed reactor; H2 and raw materials are introduced, the mass fraction of the raw material 3-hydroxybutyraldehyde aqueous solution is 40%, the reaction temperature is 100°C, the reaction time is 2h, and the mass space velocity of the raw material is 3h -1 , mass space velocity of H2 100h -1 , the reaction pressure is 3Mpa, and the hydrogenation reaction produces 1,3-butanediol.

[0082] After the reaction is stable (i.e. when the reaction spectrum data is normal), the reaction raw materials and products are analyzed by gas chromatography online. The reaction results are shown in Table 2.

[0083] Table 2

[0084]

[0085]

[0086] Example 3

[0087] Catalyst 1 prepared in Table 1 was used #The hydrogenation reaction for preparing 1,3-butanediol was carried out, and the reaction parameters were changed. Except for the parameters in Table 3, the other parameters were the same as those in Example 2. After the reaction was stable (i.e., when the reaction spectrum data was normal), the reaction raw materials and products were analyzed by gas chromatography online. The reaction results are shown in Table 3.

[0088] Table 3

[0089]

[0090] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing 1,3-butanediol by hydrogenating 3-hydroxybutyraldehyde, characterized in that: H2 and an aqueous solution containing 3-hydroxybutyraldehyde are contacted with a catalyst to react to obtain a product containing 1,3-butanediol; The catalyst comprises an active component and a carrier; The active component is NiCo2O4; The carrier is Al2O3; The active component accounts for 5-30 wt% of the mass of the catalyst, wherein the mass of the active component is calculated based on the mass of NiCo2O4; The catalyst is prepared by the following steps: (1) grinding and mixing a nickel source, a cobalt source and a solvent, drying, and calcining II to obtain NiCo2O4; In the nickel source and the cobalt source, the molar ratio of Ni element to Co element is (0.9-1):2; (2) The carrier is mixed with the NiCo2O4 obtained in step (1) and then calcined to obtain the catalyst.

2. The method according to claim 1, characterized in that The nickel source is selected from at least one of nickel nitrate, nickel sulfate and nickel acetate; The cobalt source is selected from at least one of cobalt nitrate, cobalt sulfate and cobalt acetate; The solvent is selected from one of water, ethanol, and a mixed solution of ethanol and water; The grinding time is 30 to 60 minutes.

3. The method according to claim 1, characterized in that The volume ratio of the total solid mass of the nickel source and the cobalt source to the solvent is 1: (6-7) g / ml.

4. The method according to claim 1, characterized in that: The calcination temperature is 500°C to 600°C, and the calcination time is 2h to 6h.

5. The method according to claim 1, characterized in that The drying temperature is 100°C to 120°C, and the drying time is 8h to 12h; The calcination II temperature is 800°C to 1200°C, and the calcination II time is 12h to 24h.

6. The method according to claim 1, characterized in that The mass fraction of the aqueous solution containing 3-hydroxybutyraldehyde is 20-50%; The reaction temperature of the contact reaction is 70°C to 110°C, the reaction time is 1h to 4h, and the reaction pressure is 2 to 5Mpa; The mass space velocity of the aqueous solution containing 3-hydroxybutyraldehyde is 2h -1 ~4h -1 ; The mass space velocity of H2 is 80h -1 ~120h -1 .

Citation Information

Patent Citations

  • Preparation method of 1, 3-butylene glycol

    CN109422624A

  • Preparation method of 1, 3-butylene glycol

    CN109422635A

  • Synthesis device and synthesis method of 1,3-butanediol

    CN110668917A

  • Method for preparing 1, 3-butanediol through catalytic hydrogenation

    CN111393259A

  • Hydrogenation catalyst for synthesizing 1, 3-butanediol as well as preparation method and application of hydrogenation catalyst