A modified aluminum powder based on in-situ conversion of surface oxide film into metal organic framework material and preparation method thereof
By converting the surface of aluminum powder into metal organic framework materials in situ, the problem of unchanged oxide film properties in the existing technology has been solved, and the combustion performance and energy release rate of aluminum powder have been significantly improved, providing an efficient and convenient Modification strategy, suitable for the field of energetic materials.
Patent Information
- Application Number
- CN202211405113.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-10
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-11-10
AI Technical Summary
When the existing technology improves the combustion performance and energy release characteristics of aluminum powder, the basic properties of the oxide film have not changed significantly, and the improvement in combustion energy release characteristics is limited. Most of the modification methods are external coatings, lacking efficient and convenient in-situ conversion. method.
By mixing the organic ligand dispersion and the aluminum powder dispersion at room temperature, the amphoteric characteristics of the oxide film on the surface of the aluminum powder are utilized, and under the action of alkali solution and organic acid ligands, it is converted into a metal-organic framework material in situ to form a modified Aluminum powder. The method includes dissolving an organic acid ligand in a sodium hydroxide aqueous solution and mixing it with N,N-dimethylformamide, adding it to an aluminum powder dispersion, stirring, centrifuging, washing and drying to obtain modified aluminum powder.
The combustion performance and energy release rate of aluminum powder are significantly improved, which is manifested in shortened ignition delay time, significant increase in peak pressure and boost rate, simple operation, mild conditions, low equipment requirements, superior combustion flame and violent combustion phenomenon.
Smart Images

Figure CN116140634B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of energetic materials, and in particular relates to a modified aluminum powder based on in-situ conversion of a surface oxide film into a metal organic framework material and a preparation method thereof. Background Art
[0002] Aluminum powder has high combustion calorific value (30.1kJ / g) and high density (2.7g / cm 3 ), low oxygen consumption, and abundant reserves and low manufacturing cost; as a highly active metal fuel, it is widely used in energetic materials such as aluminum-containing explosives, propellants and thermites. When the content of aluminum powder in solid propellants or explosives reaches more than 15.0wt%, it can significantly increase the specific impulse, density and combustion temperature of the propellant, and improve the explosive heat and work capacity of the explosive (Propellants Explos. Pyrotech. 2012, 37, 143–155, Prog. Energy Combust. Sci. 2017, 61, 293365). With the development of modern weapons, the comprehensive performance requirements of energetic materials are constantly increasing. Improving the energy release rate, combustion characteristics and safety performance of aluminum powder has become a research hotspot and main direction of highly active metal fuels.
[0003] Generally, the surface of aluminum powder is easily oxidized and forms an amorphous Al2O3 oxide film with a thickness of 2-6nm, which reduces the reactivity of aluminum powder. As the temperature rises, the aluminum core inside the aluminum powder melts and expands, eventually causing the oxide film to rupture, which can cause ignition; the aluminum core is fully in contact with the oxidant, and a continuous combustion reaction occurs (Combust. Flame. 2016, 169, 94-109). Therefore, the surface oxide film is an important factor affecting the combustion performance and energy release efficiency of aluminum powder. At present, surface coating is a common means to improve the combustion performance of aluminum powder. The coating materials involve fluoropolymers, carbon materials, transition metals, transition metal oxides, dopamine and polyphenols (Energetic Materials, 2020, 28, 1017-1025). Among them, the fluorine-containing gas produced by the decomposition of fluoropolymers can react with the oxide film, causing the oxide film to rupture and improve the combustion performance of aluminum powder. Chinese patents CN111217652A, CN110590483A, CN113501740A, etc., based on the interface modification strategy, polytetrafluoroethylene, heptadecafluorodecyltrimethylsilane, perfluorododecanethiol and other substances are coated on the surface of micro-nano aluminum powder to improve combustion performance. At the same time, the use of polyphenol self-polymerizing molecules such as dopamine and tannic acid to coat aluminum powder can alleviate the oxidation of aluminum powder itself, strengthen the interface between aluminum powder and oxidant, reduce particle agglomeration, and improve the reaction activity of aluminum powder (CN110550990A, CN109704896A).
[0004] Metal-organic framework materials are porous materials with regular pores. When coated on the surface of aluminum powder, they can provide abundant mass and heat transfer channels for the combustion process of aluminum powder, thereby improving the combustion performance of aluminum powder. Yan Qilong, Zou Jijun and others used dopamine and polyvinyl pyrrolidone to pre-coat nano-aluminum powder, and then adsorbed metal ions (Cu, Zn, Co, Mo); and combined with organic ligands to form aluminum-based composite fuels coated with metal-organic framework materials; thereby effectively improving the combustion performance and energy release characteristics of aluminum powder (CN109467493A, Chem. Eng. J. 2022, 430, 132909). However, the above-mentioned modification methods are all coatings of the surface of the aluminum powder oxide film with external materials. The basic properties of the oxide film have not changed significantly, and the improvement of the combustion energy release characteristics is limited. However, the Al2O3 oxide film is an amphoteric oxide, which can undergo acid-base reactions to produce metal aluminum ions (Al 3+ ); and in situ bind organic ligands on the surface to form a metal organic framework material layer (Sci. Adv. 2019, 5, eaav5340). Therefore, the in situ conversion of the oxide film on the surface of aluminum powder into a metal organic framework material can provide a more efficient and convenient method for improving the combustion energy release characteristics of aluminum powder. Summary of the invention
[0005] The purpose of the present invention is to provide a modified aluminum powder based on the in-situ conversion of the surface oxide film into a metal organic framework material and a preparation method thereof. The present invention drips and mixes an organic ligand dispersion with an aluminum powder dispersion, stirs for a period of time at room temperature, and then centrifuges, washes, and dries to obtain a modified aluminum powder in which a portion of the surface oxide film is converted into a metal organic framework material; through laser ignition, closed explosion, and thermal analysis test characterization, the modified aluminum powder has excellent combustion performance and energy release characteristics.
[0006] In order to achieve the above technical effects, the present invention provides the following technical solutions:
[0007] A method for preparing modified aluminum powder based on in-situ conversion of surface oxide film into metal organic framework material comprises the following steps:
[0008] (1) dissolving an organic acid ligand in a sodium hydroxide aqueous solution at room temperature, and then adding N,N-dimethylformamide to form an organic ligand dispersion;
[0009] (2) dispersing aluminum powder in a mixed solution consisting of water and N,N-dimethylformamide, and performing ultrasonication at room temperature to form an aluminum powder dispersion;
[0010] (3) The organic ligand dispersion is added dropwise to the aluminum powder dispersion to form an aluminum powder mixed dispersion, which is stirred at room temperature, centrifuged, washed, and dried to obtain modified aluminum powder.
[0011] A further technical solution is that the organic acid is selected from any one of terephthalic acid, trimesic acid, 2-nitroterephthalic acid, 2-aminoterephthalic acid, 2-hydroxyterephthalic acid and tetrafluoroterephthalic acid.
[0012] A further technical solution is that the aluminum powder is nano aluminum powder or micron aluminum powder, and the particle size range is 50nm to 100μm.
[0013] A further technical solution is that the volume of the organic ligand dispersion in step (3) is the same as that of the aluminum powder dispersion.
[0014] A further technical solution is that the concentration of the aluminum powder mixed dispersion in step (3) is 2.0-20.0 mg / mL, the stirring time is 5 min to 72 h, the centrifugal speed is 8000 to 12000 rpm, the washing solvent is methanol or ethanol, the drying temperature is 40 to 65°C, and the drying time is 1 to 12 h.
[0015] A further technical solution is that the ratio of the mass of the aluminum powder to the amount of the organic acid substance is 50 to 1600 mg / mmol.
[0016] The present invention also provides a modified aluminum powder prepared by the above preparation method and application of the modified aluminum powder in the field of energetic materials.
[0017] The method of the present invention utilizes the amphoteric characteristics of the oxide film on the surface of aluminum powder. Under the joint action of an alkaline solution and an organic acid ligand, the surface oxide film is in situ converted into a metal organic framework material to obtain modified aluminum powder, thereby greatly improving the combustion performance and energy release rate of the aluminum powder.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The modification method provided by the present invention mixes an organic ligand dispersion with an aluminum powder dispersion, and at room temperature, the surface oxide film of the aluminum powder can be in-situ converted into a metal organic framework material to obtain a modified aluminum powder having superior combustion performance, which is reflected in shortened ignition delay time, greatly increased peak pressure and boost rate, and violent combustion flames. The aluminum powder modification method provided by the present invention is simple to operate, mild in conditions, and has low equipment requirements. It provides a new idea and strategy for improving the energy release characteristics of metal fuels such as aluminum powder, and has considerable application prospects in the field of energetic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the XRD spectrum of the modified nano aluminum powder prepared in Example 1.
[0021] Figure 2 This is the thermal analysis spectrum of the modified nano-aluminum powder prepared in Example 1.
[0022] Figure 3 This is a diagram of the laser ignition experiment of the modified nano-aluminum powder prepared in Example 1.
[0023] Figure 4 Transmission electron microscopy and EDS element distribution diagram of the modified nano-aluminum powder prepared in Example 2.
[0024] Figure 5 This is a diagram of the laser ignition experiment of the modified nano-aluminum powder prepared in Example 2.
[0025] Figure 6 This is a diagram of the laser ignition experiment of the modified nano-aluminum powder prepared in Example 3.
[0026] Figure 7 This is a diagram of the closed explosion experiment and ignition delay time of the modified nano-aluminum powder prepared in Example 4.
[0027] Figure 8 This is a diagram of the closed explosion experiment and ignition delay time of the modified nano-aluminum powder prepared in Example 6.
[0028] Fig. 9 This is the thermal analysis spectrum of the modified micron aluminum powder prepared in Example 7.
[0029] Fig.10 This is the thermal analysis spectrum of the modified micron aluminum powder prepared in Example 8. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is described below in conjunction with specific examples, but the protection scope of the present invention is not limited thereto.
[0031] Example 1
[0032] In this example, 1.0g of nano aluminum powder (80nm) was dispersed in a mixed solution of 50mL water and 50mL N,N-dimethylformamide (DMF), and ultrasonicated for 20min to form an aluminum powder dispersion. At the same time, 20mmol (3.3562g) of terephthalic acid was dissolved in a solution consisting of 40mmol (1.6667g) of sodium hydroxide and 50mL of water. After it was completely dissolved, 50mL of DMF was added to form an organic ligand dispersion. Subsequently, the organic ligand dispersion was added dropwise to the aluminum powder dispersion under stirring for 15min; after the addition was completed, the concentration of the aluminum powder was 5mg / mL, and it was stirred at room temperature for 10min, 30min, 60min and 120min respectively, and the modified nano aluminum powder was obtained by centrifugation, ethanol washing, and drying at 65℃ for 4h. In this example, the ratio of the mass of aluminum powder (mg) to the amount of organic acid substance (mmol) is 50, and the obtained modified aluminum powders are marked as n-Al-50-10, n-Al-50-30, n-Al-50-60, and n-Al-50-120, respectively.
[0033] Figure 1 The XRD spectrum of the modified nano aluminum powder obtained in this example. Compared with the unmodified nano aluminum powder, the modified nano aluminum powder has obvious crystal diffraction peaks of MIL-53 aluminum-containing metal organic framework materials in the range of 5-35 degrees, and maintains the diffraction peak of metal aluminum in the range of 35-90 degrees. This shows that the surface of the modified nano aluminum powder contains metal organic framework materials. Figure 2 The thermal analysis spectrum of modified nano-aluminum powder. In differential scanning calorimetry analysis, the modified nano-aluminum powder showed two exothermic peaks, corresponding to the decomposition of the surface organic framework material and the surface oxidation of the nano-aluminum powder, which produced obvious CO2 mass spectrum peaks. This further proves that after modification, the surface of the nano-aluminum powder is converted into a metal organic framework material. Figure 3 This is the laser ignition test diagram of the modified nano-aluminum powder obtained in this example. The laser ignition test conditions are 50 mg of stacked powder, 60 W of laser power, and 1 second of action time. Figure 3 It can be seen that the flame brightness of the modified nano-aluminum powder is stronger than that of the unmodified nano-aluminum powder, and it shows a distinct inner flame and outer flame structure, and the time to reach the maximum flame brightness gradually decreases from 780ms to 461ms. It can be seen that the modified nano-aluminum powder containing metal organic framework materials has better combustion performance.
[0034] Example 2
[0035] In this example, 1.0g of nano aluminum powder (80nm) was dispersed in a mixed solution of 50mL water and 50mL N,N-dimethylformamide (DMF), and ultrasonicated for 10min to form an aluminum powder dispersion. At the same time, 10mmol (1.6781g) of terephthalic acid was dissolved in a solution consisting of 20mmol (0.8335g) sodium hydroxide and 50mL water. After it was completely dissolved, 50mL DMF was added to form an organic ligand dispersion. Subsequently, the organic ligand dispersion was added dropwise to the aluminum powder dispersion under stirring for 10min; after the addition was completed, the concentration of the aluminum powder was 5mg / mL, and it was stirred at room temperature for 10min, 30min, 60min and 120min respectively, and the modified nano aluminum powder was obtained by centrifugation, ethanol washing, and drying at 65℃ for 4h. In this example, the ratio of the mass of aluminum powder (mg) to the amount of organic acid substance (mmol) is 100, and the obtained modified aluminum powders are marked as n-Al-100-10, n-Al-100-30, n-Al-100-60, and n-Al-100-120, respectively.
[0036] Figure 4The transmission electron microscope image of n-Al-100-10 directly shows that a layer of metal organic framework material is formed on the surface of the modified nano aluminum powder, and its lattice fringes are clearly visible, which is obviously different from the amorphous Al2O3 oxide film on the surface of the unmodified nano aluminum powder. In the EDS element distribution, the C element from the organic ligand is distributed on the surface of the modified nano aluminum powder, forming an obvious core-shell structure, which further illustrates that the method provided by the present invention can in-situ convert the surface oxide film of the nano aluminum powder into a metal organic framework material. Figure 5 This is the laser ignition test picture of the modified nano aluminum powder obtained in this example. It can be seen that the modified nano aluminum powders all present a brighter combustion flame. In addition, n-Al-100-10 presents a micro-explosion combustion experimental phenomenon, the combustion process is intense, and the combustion performance of the modified nano aluminum powder is greatly improved.
[0037] Example 3
[0038] In this example, 1.0g of nano aluminum powder (80nm) was dispersed in a mixed solution of 50mL water and 50mL N,N-dimethylformamide (DMF), and ultrasonicated for 10min to form an aluminum powder dispersion. At the same time, 5mmol (0.8391g) of terephthalic acid was dissolved in a solution consisting of 10mmol (0.4167g) of sodium hydroxide and 50mL of water. After it was completely dissolved, 50mL of DMF was added to form an organic ligand dispersion. Subsequently, the organic ligand dispersion was added dropwise to the aluminum powder dispersion under stirring for 10min; after the addition was completed, the concentration of the aluminum powder was 5mg / mL, and it was stirred at room temperature for 10min, 30min, 60min and 120min respectively, and the modified nano aluminum powder was obtained by centrifugation, ethanol washing, and drying at 65℃ for 4h. In this example, the ratio of the mass of aluminum powder (mg) to the amount of organic acid substance (mmol) is 200, and the obtained modified aluminum powders are marked as n-Al-200-10, n-Al-200-30, n-Al-200-60, and n-Al-200-120, respectively.
[0039] Figure 6 This is the laser ignition test picture of the modified nano aluminum powder obtained in this example. Compared with the unmodified nano aluminum powder, the modified nano aluminum powder also presents a brighter combustion flame. In addition, n-Al-200-30 and n-Al-200-120 show micro-explosion combustion phenomenon, and the combustion performance of the modified nano aluminum powder is greatly improved.
[0040] Example 4
[0041] In this example, 1.0g of nano-aluminum powder (80nm) was dispersed in a mixed solution of water and N,N-dimethylformamide (DMF) with a volume of 100mL, and ultrasonicated for 10min to form an aluminum powder dispersion. At the same time, 10mmol (1.6781g) of terephthalic acid was dissolved in a mixed solution of water and N,N-dimethylformamide (DMF) containing 20mmol (0.8335g) of sodium hydroxide with a volume of 100mL to form an organic ligand dispersion. Subsequently, the organic ligand dispersion was added dropwise to the aluminum powder dispersion under stirring for 15min; after the addition was completed, the total volume of the aluminum powder mixed dispersion was 200mL, and the aluminum powder concentration was 5mg / mL. In this example, the volume ratio of DMF and water was adjusted to DMF (mL) / H2O (mL) = 175 / 25, 150 / 150, 100 / 100, 50 / 150, 25 / 175, 0 / 200, respectively, and the total volume of the mixed dispersion was maintained at 200 mL. The mixture was stirred at room temperature for 10 min, and then centrifuged, washed with ethanol, and dried at 65°C for 4 h to obtain a series of modified nano aluminum powders.
[0042] In this example, 200 mg of nano-aluminum powder was placed in a 330 mL sealed container. The nano-aluminum powder was ignited by a nickel-chromium wire under 1 MPa oxygen. The pressurization curve of the aluminum powder combustion process was recorded, and the peak pressure and pressurization rate were calculated; the ignition delay time was obtained by the laser ignition experiment. Figure 7 The results of the closed explosion experiment and ignition delay time of the modified nano aluminum powder obtained in this example. Compared with the unmodified nano aluminum powder, the peak pressure and the pressurization rate of the modified nano aluminum powder are improved. When DMF (mL) / H2O (mL) = 100 / 100, the modified nano aluminum powder shows a better peak pressure and pressurization rate. At the same time, the ignition delay time of the modified nano aluminum powder is greatly reduced and shortened to 10ms. The closed explosion and ignition delay time results show that the method of the present invention effectively improves the combustion performance and energy release rate of nano aluminum powder.
[0043] Example 5
[0044] In this example, the combustion performance of the modified nano aluminum powder can be adjusted by changing the amount of sodium hydroxide. The specific operation steps are as follows: 1.0g of nano aluminum powder (80nm) is dispersed in a mixed solution of 50mL water and 50mL N,N-dimethylformamide (DMF), and ultrasonicated for 10min to form an aluminum powder dispersion. At the same time, 10mmol (1.6781g) of terephthalic acid is dissolved in 50mL of sodium hydroxide aqueous solution. After it is completely dissolved, 50mL of DMF is added to form an organic ligand dispersion. The amount of sodium hydroxide is 10, 20, 30, and 40mmol. Subsequently, the organic ligand dispersion is added dropwise to the aluminum powder dispersion under stirring, and the addition time is 10min; after the addition is completed, the concentration of the aluminum powder is 5mg / mL, and it is stirred at room temperature for 30min, centrifuged, washed with ethanol, and dried at 65℃ for 4h to obtain a series of modified nano aluminum powders.
[0045] From the perspective of closed explosion experiments, laser ignition experiments and ignition delay time, when the dosage of sodium hydroxide is 20 mmol, the modified nano-aluminum powder has better combustion performance and energy release characteristics.
[0046] Example 6
[0047] This example modulates the combustion performance of modified nano aluminum powder by changing the type of organic ligand. The specific operation steps are as follows: 1.0g of nano aluminum powder (80nm) is dispersed in a mixed solution of 50mL water and 50mL N,N-dimethylformamide (DMF), and ultrasonicated for 10min to form an aluminum powder dispersion. At the same time, 10mmol of substituted terephthalic acid is dissolved in 50mL of sodium hydroxide aqueous solution. After it is completely dissolved, 50mL of DMF is added to form an organic ligand dispersion. The amount of sodium hydroxide used is 20mmol (0.8335g). Substituted terephthalic acid includes 2-nitroterephthalic acid (-NO2), 2-aminoterephthalic acid (-NH2), 2-hydroxyterephthalic acid (-OH) and tetrafluoroterephthalic acid (-4F). Subsequently, the organic ligand dispersion was added dropwise to the aluminum powder dispersion under stirring for 10 min. After the addition, the concentration of the aluminum powder was 5 mg / mL. The mixture was stirred at room temperature for 30 min, and then centrifuged, washed with ethanol, and dried at 65°C for 4 h to obtain a series of modified nano aluminum powders.
[0048] Figure 8 The results of the closed explosion experiment and ignition delay time of the modified nano-aluminum powder obtained in this example. Compared with the unmodified nano-aluminum powder, the modified nano-aluminum powders obtained using different organic ligands all showed higher peak pressure and pressurization rate, and had a faster energy release rate. In terms of ignition delay time, the modified nano-aluminum powder obtained by terephthalic acid had the shortest ignition delay time; the ignition delay time of other modified nano-aluminum powders showed a shortening trend.
[0049] Example 7
[0050] In this example, 1.6781g of sodium hydroxide was dissolved in 25mL of water, and 0.9263g of terephthalic acid was added. After it was completely dissolved, 25mL of DMF was added to form an organic ligand dispersion. At the same time, 0.5g of micron aluminum powder (10±2μm) was dispersed in a mixed solution of 25mL of water and 25mL of DMF, and ultrasonicated for 10 minutes to form an aluminum powder dispersion. Subsequently, the organic ligand dispersion was added dropwise to the aluminum powder dispersion under stirring at a speed of 600rpm, and the addition time was about 10 minutes; after the addition was completed, the concentration of the aluminum powder was 5mg / mL, and it was stirred at room temperature for 2h. Finally, this example obtained modified micron aluminum powder by centrifugation, ethanol washing, and drying at 65℃ for 4h.
[0051] The TG-DSC-MS analysis of the micron aluminum powder and the modified micron aluminum powder of this example are shown in Fig. 9 a and Fig. 9 b. By Fig. 9 It can be seen from a that the oxidation weight gain of micron aluminum powder is about 19.5%, the DSC exothermic peak temperature is 1012.9℃, and the heat release is 4179J / g. Fig. 9 b It can be seen that the oxidation weight gain of the modified micron aluminum powder is about 50.3%, the DSC exothermic peak temperature is 1015.9℃, and the heat release is 12182J / g, which is about three times increased. The modified micron aluminum powder has a small weight loss at 600℃, and releases a large amount of CO2 (m / z=44), which corresponds to the decomposition of the metal organic framework material on the surface of the modified micron aluminum powder. In short, the energy release efficiency of the modified micron aluminum powder is greatly improved.
[0052] Example 8
[0053] In this example, 0.674g of sodium hydroxide was dissolved in 25mL of water, and 1.072g of trimesic acid was added. After it was completely dissolved, 25mL of DMF was added to form an organic ligand dispersion. At the same time, 0.5g of micron aluminum powder (10±2μm) was dispersed in a mixed solution of 25mL of water and 25mL of DMF, and ultrasonicated for 10 minutes to form an aluminum powder dispersion. Subsequently, the organic ligand dispersion was added dropwise to the aluminum powder dispersion under stirring at a speed of 600rpm, and the dropping time was about 10 minutes; after the addition was completed, the concentration of the aluminum powder was 5mg / mL, and it was stirred at room temperature for 3d. Finally, this example obtained modified micron aluminum powder by centrifugation, ethanol washing, and drying at 65°C for 4h, and its TG-DSC-MS showed Fig.10 In addition, in this example, the amount of solvent was halved. After the addition was completed, the concentration of aluminum powder was 10 mg / mL. Other conditions remained unchanged. Modified micron aluminum powder was also obtained. Its TG-DSC-MS showed Fig.10 b.
[0054] Depend on Fig.10 It can be seen from a that when the concentration of aluminum powder is 5 mg / mL, the oxidation weight gain of the modified micron aluminum powder is about 21.4%, the DSC exothermic peak temperature is 954.5℃, the heat release is about 60℃ in advance, and the heat release is 7343J / g; Fig.10 b shows that when the concentration of aluminum powder is 10 mg / mL, the DSC exothermic peak temperature is 981.3℃, which is about 31.6℃ in advance, and the heat release is 4275 J / g. Therefore, trimesic acid, as an organic ligand, forms a metal organic framework material on the surface of micron aluminum powder, which can promote the early heat release of micron aluminum powder, increase the heat release, and improve the energy release rate of micron aluminum powder.
[0055] From the above examples, it can be seen that the modified aluminum powder and preparation method based on the in-situ conversion of the surface oxide film into the metal frame material provided by the present invention are simple to operate, mild conditions, and can achieve the modification of micro-nano aluminum powder at room temperature, greatly improving the combustion performance and energy release rate of micro-nano aluminum powder. The metal fuel modification method provided by the present invention is efficient, convenient, environmentally friendly, has low equipment requirements, and has considerable application prospects in the field of energetic materials.
[0056] Although the present invention is described herein with reference to the illustrative embodiments of the present invention, the above embodiments are only preferred embodiments of the present invention, and the embodiments of the present invention are not limited to the above embodiments. It should be understood that those skilled in the art can design many other modifications and embodiments, which will fall within the scope and spirit of the principles disclosed in this application.
Claims
1. A method for preparing modified aluminum powder based on in-situ conversion of surface oxide film into metal organic framework material, characterized in that: The following steps are involved: (1) dissolving an organic acid ligand in a sodium hydroxide aqueous solution at room temperature, and then adding N,N-dimethylformamide to form an organic ligand dispersion; the organic acid is selected from any one of terephthalic acid, trimesic acid, 2-nitroterephthalic acid, 2-aminoterephthalic acid, 2-hydroxyterephthalic acid and tetrafluoroterephthalic acid; (2) dispersing aluminum powder in a mixed solution consisting of water and N,N-dimethylformamide, and mixing by ultrasonication at room temperature to form an aluminum powder dispersion; the aluminum powder is nano aluminum powder or micron aluminum powder, and the particle size ranges from 50 nm to 100 μm; (3) adding the organic ligand dispersion to the aluminum powder dispersion to form an aluminum powder mixed dispersion, stirring at room temperature, centrifuging, washing, and drying to obtain modified aluminum powder; the organic ligand dispersion has the same volume as the aluminum powder dispersion; the concentration of the aluminum powder mixed dispersion is 2.0-20.0 mg / mL; and the ratio of the mass of the aluminum powder to the amount of the organic acid substance is 50-1600 mg / mmol.
2. The method for preparing modified aluminum powder based on in-situ conversion of surface oxide film into metal organic framework material according to claim 1, characterized in that: In step (3), the stirring time is 5 min to 72 h, the centrifugal speed is 8000 to 12000 rpm, the washing solvent is methanol or ethanol, the drying temperature is 40 to 65° C., and the drying time is 1 to 12 h.
3. A modified aluminum powder, characterized in that: The preparation method is described in any one of claims 1 to 2.
4. Use of the modified aluminum powder according to claim 3 in the field of energetic materials.
Citation Information
Patent Citations
Preparation method of metal-organic framework material modified metal nanoparticles
CN109467493A
Polydopamine interface regulation-based nitramine explosive modified aluminum powder and preparation method thereof
CN109704896A
Preparation method of polymerized tannic acid coated high-activity aluminium powder / silicon powder
CN110550990A
Method for preparing fluorine-containing compound coated micro-nano aluminum powder
CN110590483A
Composite solid propellant based on fluorine polymer modified aluminum powder, and preparation method thereof
CN111217652A