A heat-resistant coating for thermal transfer carbon ribbon and its preparation method and coating process

By crosslinking polymer chains such as titanium acetylacetone with materials such as α,ω-dihydroxypolysiloxane, a thermal transfer carbon tape coating with higher heat resistance and adhesion is prepared, and the existing technology is solved The problem of insufficient heat resistance and adhesion properties of medium heat-resistant coating materials has improved the printing temperature level and production speed.

CN116144261BActive Publication Date: 2024-11-22福建鸣友新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210983152.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-11-22
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

The heat resistance and adhesion performance of existing thermal transfer carbon tape heat-resistant coating materials are insufficient, resulting in easy strip breakage and cassette breakage under high temperature continuous printing conditions.

Method used

Heat-resistant coating materials are prepared by mixing polymer chains such as titanium acetylacetone and hydroxyl groups with α,ω-dihydroxypolysiloxane, methacryloyloxypropyltrimethoxysilane and dibutyltin dilaurate. , and the adhesion to the PET base film is improved through cross-linking reaction.

Benefits of technology

It significantly improves the high temperature resistance and adhesion of the thermal transfer carbon belt, reduces the probability of base film melting and breaking during printing, and improves the printing temperature and production speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116144261B_ABST
    Figure CN116144261B_ABST
Patent Text Reader

Abstract

The invention discloses a heat-resistant coating for thermal transfer ribbon, which is prepared by mixing titanium acetylacetonate, α,ω-dihydroxy polysiloxane with hydroxyl as terminal group, methacryloxypropyl trimethoxy silane, dibutyl tin dilaurate, and an organic solvent. The present invention mixes titanium acetylacetonate into the polymer chain of organic substances such as α,ω-dihydroxy polysiloxane with hydroxyl as terminal group, methacryloxypropyl trimethoxy silane, dibutyl tin dilaurate, etc., thereby improving the activation energy of the polymer chain, so that the degradation of the polymer chain needs to overcome a higher energy barrier, absorb more energy, and effectively improve the high temperature resistance of the heat-resistant coating for thermal transfer ribbon. The heat-resistant coating for thermal transfer ribbon obtained has good high temperature resistance, strong adhesion to the base film, and reduces the probability of the base film melting and breaking during printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a heat-resistant coating of a thermal transfer carbon ribbon and a preparation method and a coating process thereof, belonging to the technical field of thermal transfer carbon ribbons. Background Art

[0002] Thermal digital printers use thermal transfer ribbons to transfer specific information carriers to substrates to form QR codes, barcodes, pictures, text, etc. Thermal transfer technology is widely used in many fields such as modern bills, clothing labels, pharmaceutical packaging, and manufacturing. Due to its automatic recognition function, it has a wide range of uses and large usage.

[0003] The transfer ribbon is the core material in the operation of the thermal transfer printer. It consists of four parts: heat-resistant coating, PET base film, primer, and ink. During thermal transfer, the ribbon will be subjected to instantaneous high temperature and pressure from the thermal head of the printer. The ribbon base is a PET film of 4.5μm to 6μm, and the PET film begins to deform at around 210°C. Under the combined effect of high temperature and tensile force, the base film of the ribbon product is easy to melt and break. In order to ensure the printing effect, it is necessary to apply a heat-resistant coating on the back of the base film. In actual production, the following requirements are imposed on this heat-resistant coating: it must have high heat resistance to ensure that the PET substrate is not damaged when it contacts the thermal print head, and the friction coefficient must be small when in contact with the thermal head to ensure a smooth transfer process. The heat-resistant coating must also have good adhesion to the PET base film to ensure that the thermal head is not contaminated during printing.

[0004] In recent years, reports on the environmental performance and printing performance of thermal transfer ribbons have shown explosive growth. The invention patent "Thermal transfer ribbon suitable for printing bills" (CN201910930458.X) reports a thermal transfer ribbon used in the bill printing process. The residual ink layer after printing can be easily scraped off, and the base tape does not leave any printing marks. The invention patent "An ionic liquid modified barcode carbon ribbon back coating coating and its preparation method" (CN201810674167.4) reports that by block polymerization, the polyacrylate back coating polymer chain is introduced into an ionic liquid containing double bonds to produce a low-resistivity polymer heat-resistant coating material and coat the barcode carbon ribbon, thereby improving the printing quality of the thermal transfer ribbon. However, the above patent still has the problem of insufficient heat resistance and adhesion performance of the heat-resistant coating material. The phenomenon of broken tape and jamming occurs under the production conditions of high-temperature continuous printing. The heat resistance and adhesion of the heat-resistant coating material need to be improved. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a heat-resistant coating for a thermal transfer carbon ribbon, a preparation method and a coating process thereof. By mixing titanium acetylacetonate into polymer chains of α,ω-dihydroxypolysiloxane, methacryloxypropyltrimethoxysilane, dibutyltin dilaurate, etc. with hydroxyl groups as end groups, the activation energy of the polymer chain is increased, so that the polymer chain needs to overcome a higher energy barrier when degrading and absorbs more energy, thereby effectively improving the high temperature resistance of the heat-resistant coating for the thermal transfer carbon ribbon.

[0006] The present invention is achieved through the following scheme: a heat-resistant coating for a thermal transfer carbon ribbon and a preparation method and coating process thereof, which is prepared by mixing titanium acetylacetonate, α,ω-dihydroxypolysiloxane with hydroxyl groups as terminal groups, methacryloxypropyltrimethoxysilane, dibutyltin dilaurate, and an organic solvent.

[0007] The contents of the above-mentioned components are as follows: in parts by weight, 1 to 3 parts of titanium acetylacetonate, 200 to 220 parts of α,ω-dihydroxypolysiloxane with hydroxyl groups as terminal groups, 18 to 22 parts of methacryloxypropyltrimethoxysilane, 2.8 parts of dibutyltin dilaurate, and 7850 to 8850 parts of an organic solvent.

[0008] The organic solvent is one or more of xylene, butanone and cyclohexanone.

[0009] A method for preparing a heat-resistant coating of a thermal transfer carbon ribbon comprises the following steps:

[0010] Step 1, weighing titanium acetylacetonate, α,ω-dihydroxy polysiloxane with hydroxyl groups as terminal groups, methacryloxypropyltrimethoxysilane, and an organic solvent, stirring at room temperature for 40 to 60 hours to obtain an organic solution of titanium acetylacetonate;

[0011] Step 2, adding an organic solvent to the solution obtained in step 1 and stirring for 2 to 4 hours;

[0012] Step 3, weigh dibutyltin dilaurate and add an organic solvent thereto, and stir at room temperature for 15 minutes;

[0013] Step 4: Add the solution obtained in step 3 to the solution obtained in step 2, and stir for 10 to 20 minutes to obtain the thermal transfer carbon ribbon heat-resistant coating material.

[0014] A coating process for a heat-resistant coating of a thermal transfer carbon ribbon comprises the following steps:

[0015] Step 1: The driving shaft drives the PET base film to move, the coating plate is fixed, and the heat-resistant coating material of the thermal transfer carbon ribbon is evenly coated on the surface of the PET base film;

[0016] Step 2: Use a smoothing device to scrape off excess heat-resistant coating material on the surface of the PET base film to ensure a consistent coating thickness;

[0017] Step 3: The driving shaft drives the PET base film coated with the heat-resistant coating material horizontally through a 15-meter-long oven to evaporate the solvent. The titanium acetylacetonate undergoes a cross-linking reaction with the active groups such as -OH, -NH2, and -CONH2 in the PET base film to increase the molecular weight and improve the adhesion between the heat-resistant coating material and the PET substrate. The film is then transported out through another driving shaft.

[0018] The smoothing device used in the step 2 includes a device body, a smoothing guide roller, a scraper mechanism and a flattening roller. The smoothing guide roller, the scraper mechanism and the flattening roller are all arranged inside the device body. A pad is also provided inside the device body. The smoothing guide roller is located on the front side of the pad, the scraper mechanism and the flattening roller are located on the upper side of the pad, and the flattening roller is located on the rear side of the scraper mechanism. The PET base film with a heat-resistant coating passes through the smoothing guide roller, between the scraper mechanism and the pad, and between the flattening roller and the pad in sequence.

[0019] The scraper mechanisms are provided with two, which are arranged front and back and run in turns.

[0020] The scraper mechanism includes a paint collecting box, a central axis and a scraper. A connecting plate is provided on the front side of the paint collecting box. The central axis vertically passes through the connecting plate. The front and rear ends of the central axis are connected to the front and rear side walls of the device body. The scraper is connected to the lower end of the connecting plate. A paint collection inlet is provided between the upper end of the connecting plate and the upper side wall of the paint collecting box.

[0021] The central axis drives the connecting plate, the paint collecting box and the scraper to rotate under the control of the control device. The scraper is a curved surface structure, and the front side of the connecting plate is a slope structure.

[0022] In the step 3, the movement speed of the PET base film coated with the heat-resistant coating material in the oven is 290-310 m / min, and the drying temperature is 105-115°C.

[0023] The beneficial effects of the present invention are:

[0024] 1. The present invention adds titanium acetylacetonate to α,ω-dihydroxy polysiloxane with hydroxyl groups as terminal groups, methacryloxypropyl trimethoxysilane, and dibutyltin dilaurate to prepare a heat-resistant coating material, and after the prepared heat-resistant coating material is coated on the surface of the PET base film, the effective printing temperature of the carbon ribbon can be increased to 128°C, which exceeds the high temperature resistance of 125°C of the imported carbon ribbon, and significantly reduces the probability of the base film melting and breaking during the printing process;

[0025] 2. The conveyor wheel of the present invention drives the coated PET base film to pass through the oven, which greatly improves the drying speed and production speed of the heat-resistant coating. At the same time, after the solvent evaporates, titanium acetylacetonate can react with active groups such as -OH, -NH2, and -CONH2 in the PET base film to form a bridge, thereby increasing the molecular weight and improving the adhesion between the heat-resistant coating material and the PET substrate;

[0026] 3. The process of the present invention is simple and meets the needs of the actual production process of the factory. The performance of the heat-resistant coating of the thermal transfer carbon ribbon is improved while also improving the competitiveness of the enterprise.

[0027] 4. Two scraper mechanisms are arranged in the smoothing device of the present invention. When one is in operation, the other can clean the attachments on the scraper. They are also standby for each other. If one is broken, the other can also be used, thus ensuring the stability of the rectification and smoothing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a schematic diagram of the process structure of a coating process for a heat-resistant coating of a thermal transfer carbon ribbon.

[0029] Figure 2 The present invention is a schematic diagram of a front view cross-sectional structure of a smoothing device in a coating process of a heat-resistant coating of a thermal transfer carbon ribbon.

[0030] Figure 3 The present invention is a schematic diagram of a front cross-sectional structure of a scraper mechanism in a coating process of a heat-resistant coating layer of a thermal transfer carbon ribbon when in use.

[0031] Figure 4 The present invention is a schematic diagram of a front cross-sectional structure of a scraper mechanism in a coating process of a heat-resistant coating of a thermal transfer carbon ribbon when not in use.

[0032] Figure 5 Schematic diagram of the cross-linking of titanium acetylacetonate and the active group (-OH) of α,ω-dihydroxypolysiloxane.

[0033] In the figure: 1 is a driving shaft, 2 is a PET base film, 3 is a smoothing device, 4 is an oven, 5 is a device body, 6 is a smoothing guide roller, 7 is a scraper mechanism, 8 is a flattening roller, 9 is a pad, 10 is a paint collecting box, 11 is a central shaft, 12 is a scraper, 13 is a connecting plate, and 14 is a paint collecting inlet. DETAILED DESCRIPTION

[0034] Combine the following Figure 1-5 The present invention is further described, but the protection scope of the present invention is not limited to the described contents.

[0035] The same parts are denoted by the same reference numerals. It should be noted that the words "front", "rear", "left", "right", "upper" and "lower" used in the following description refer to directions in the drawings, and the words "inner" and "outer" refer to directions toward or away from the geometric center of a specific component, respectively. The drawings are all in very simplified form and use inaccurate ratios, which are only used to facilitate and clearly assist in explaining the purpose of the embodiments of the present invention.

[0036] For the sake of clarity, not all features of an actual embodiment are described. In the following description, well-known functions and structures are not described in detail because they would obscure the invention with unnecessary detail. It should be recognized that in the development of any actual embodiment, a large number of implementation details must be made to achieve the specific goals of the developer, such as changing from one embodiment to another according to relevant system or relevant business limitations. In addition, it should be recognized that such development work may be complex and time-consuming, but it is merely routine work for those skilled in the art.

[0037] Example 1: Preparation method of heat-resistant coating material for thermal transfer carbon ribbon (the organic solvent is xylene).

[0038] Step 1, weigh 1 g of titanium acetylacetonate, 200 g of α,ω-dihydroxypolysiloxane with hydroxyl groups as terminal groups, 18 g of methacryloxypropyltrimethoxysilane, and 1000 g of xylene, mix them well, and stir at room temperature for 40 hours to obtain an organic solution of titanium acetylacetonate;

[0039] Step 2: Add 2000 g of xylene to the solution obtained in step 1 and stir for 2 hours;

[0040] Step 3, weigh 2.8 g of dibutyltin dilaurate and add 4850 g of xylene thereto, and stir at room temperature for 15 minutes;

[0041] Step 4: Add the solution obtained in step 3 to the solution obtained in step 2, and stir for 10 minutes to obtain the thermal transfer carbon ribbon heat-resistant coating material.

[0042] The heat-resistant coating material prepared in Example 1 was applied to the coating process shown in Example 6. The thermal transfer ribbon prepared was able to increase the effective printing temperature of the ribbon to 128°C set in the Citizen printer S621C when full black printing was adopted. There were no defects on the label paper and no cracks on the PET base film. 62 sheets could be printed per minute during continuous printing.

[0043] Example 2: Preparation method of heat-resistant coating material of thermal transfer carbon ribbon (the organic solvent is butanone).

[0044] Step 1, weigh 2 g of titanium acetylacetonate, 210 g of α,ω-dihydroxypolysiloxane with hydroxyl groups as terminal groups, 20 g of methacryloxypropyltrimethoxysilane, and 2000 g of butanone, and stir at room temperature for 50 hours to obtain an organic solution of titanium acetylacetonate;

[0045] Step 2: Add 2000 g of butanone to the solution obtained in step 1 and stir for 3 hours;

[0046] Step 3: Weigh 2.8 g of dibutyltin dilaurate, add 4000 g of butanone, and stir at room temperature for 15 minutes;

[0047] Step 4: Add the solution obtained in step 3 to the solution obtained in step 2, and stir for 15 minutes to obtain the thermal transfer carbon ribbon heat-resistant coating material.

[0048] The heat-resistant coating material prepared in Example 2 was applied to the coating process shown in Example 7 to obtain a thermal transfer ribbon with full black printing: the effective printing temperature of the ribbon can be increased to 128°C set in the Citizen printer S621C, and there are no defects on the label paper and no cracks on the PET base film. 63 sheets can be printed per minute during continuous printing.

[0049] Example 3: Preparation method of heat-resistant coating material for thermal transfer carbon ribbon (the organic solvent is cyclohexanone).

[0050] Step 1, weigh 3 g of titanium acetylacetonate, 220 g of α,ω-dihydroxypolysiloxane with hydroxyl groups as terminal groups, 22 g of methacryloxypropyltrimethoxysilane, and 1500 g of cyclohexanone, and stir at room temperature for 60 hours to obtain an organic solution of titanium acetylacetonate;

[0051] Step 2: Add 1500 g of cyclohexanone to the solution obtained in step 1 and stir for 4 hours;

[0052] Step 3, weigh 2.8 g of dibutyltin dilaurate and add 5850 g of cyclohexanone thereto, and stir at room temperature for 15 minutes;

[0053] Step 4: Add the solution obtained in step 3 to the solution obtained in step 2, and stir for 20 minutes to obtain the thermal transfer carbon ribbon heat-resistant coating material.

[0054] The heat-resistant coating material prepared in Example 3 was applied to the coating process shown in Example 8 to obtain a thermal transfer ribbon for full black printing: the effective printing temperature of the ribbon can be increased to 128°C set in the Citizen printer S621C, and there are no defects on the label paper and no cracks on the PET base film. 65 sheets can be printed per minute during continuous printing.

[0055] Example 4: Preparation method of heat-resistant coating material of thermal transfer carbon ribbon (the organic solvent is butanone and cyclohexanone).

[0056] Step 1, weigh 3 g of titanium acetylacetonate, 220 g of α,ω-dihydroxypolysiloxane with hydroxyl groups as terminal groups, 22 g of methacryloxypropyltrimethoxysilane, 1000 g of butanone, and 1000 g of cyclohexanone, and stir at room temperature for 60 hours to obtain an organic solution of titanium acetylacetonate;

[0057] Step 2: Add 1500 g each of butanone and cyclohexanone to the solution obtained in step 1 and stir for 4 hours;

[0058] Step 3, weigh 2.8 g of dibutyltin dilaurate and add 1900 g each of butanone and cyclohexanone thereto, and stir at room temperature for 15 minutes;

[0059] Step 4: Add the solution obtained in step 3 to the solution obtained in step 2, and stir for 20 minutes to obtain the thermal transfer carbon ribbon heat-resistant coating material.

[0060] The heat-resistant coating material prepared in Example 4 was applied to the coating process shown in Example 9 to obtain a thermal transfer ribbon for full black printing: the effective printing temperature of the ribbon can be increased to 128°C set in the Citizen printer S621C, and there are no defects on the label paper and no cracks on the PET base film. 65 sheets can be printed per minute during continuous printing.

[0061] Example 5: Preparation method of heat-resistant coating material of thermal transfer carbon ribbon (the organic solvents are xylene and butanone).

[0062] Step 1, weigh 2.5 g of titanium acetylacetonate, 210 g of α,ω-dihydroxypolysiloxane with hydroxyl groups as terminal groups, 20 g of methacryloxypropyltrimethoxysilane, 1000 g of xylene, and 1000 g of butanone, and stir at room temperature for 50 hours to obtain an organic solution of titanium acetylacetonate;

[0063] Step 2: Add 1000 g of xylene and 1000 g of butanone to the solution obtained in step 1 and stir for 3 hours;

[0064] Step 3, weigh 2.8 g of dibutyltin dilaurate, add 2000 g of xylene and 2000 g of butanone, and stir at room temperature for 15 minutes;

[0065] Step 4: Add the solution obtained in step 3 to the solution obtained in step 2, and stir for 15 minutes to obtain the thermal transfer carbon ribbon heat-resistant coating material.

[0066] The heat-resistant coating material prepared in Example 5 was applied to the coating coating process shown in Example 10 to obtain a thermal transfer ribbon. When full black printing is used, the effective printing temperature of the ribbon can be increased to 128°C set in the Citizen printer S621C, and there are no defects on the label paper and no cracks on the PET base film. 65 sheets can be printed per minute during continuous printing.

[0067] Example 6: Coating process of heat-resistant coating of thermal transfer carbon ribbon.

[0068] The driving shaft drives the PET base film to move, and the carbon belt speed is 290 meters / minute. The coating plate is fixed, and the heat-resistant coating material of the thermal transfer carbon belt prepared in Example 1 is uniformly conveyed thereto and uniformly coated on the surface of the PET base film. A smoothing device is used to scrape off the excess heat-resistant coating material on the surface of the PET base film to ensure consistent coating thickness. The PET base film coated with the heat-resistant coating material passes through a 15-meter-long oven at a speed of 290 meters / minute to improve the bonding performance of the heat-resistant coating material and the PET base film, wherein the oven temperature is 105°C. During the smoothing process, one of the scraper mechanisms 7 is controlled to operate, and the other scraper mechanism 7 is rotated 90 degrees. After a certain amount of waste material is removed from the scraper 12, the central axis 11 rotates 90 degrees, and the scraped material can enter the paint collection box 10 from the paint collection inlet 14 for use. The two scraper mechanisms 7 operate in turn, and one recycles the material while the other is operating.

[0069] The heat-resistant coating material prepared in Example 2 was applied to the heat-resistant coating coating process of Example 6. When the thermal transfer carbon ribbon was printed in full black, the effective printing temperature of the carbon ribbon could be increased to 128°C set in the Citizen printer S621C, and there were no defects on the label paper and no cracks on the PET base film. 63 sheets could be printed per minute during continuous printing.

[0070] Example 7: Coating process of heat-resistant coating of thermal transfer carbon ribbon.

[0071] The driving shaft drives the PET base film to move, and the carbon belt speed is 300 meters / minute. The coating plate is fixed, and the heat-resistant coating material prepared in Example 2 is uniformly conveyed thereto and uniformly coated on the surface of the PET base film. A smoothing device is used to scrape off the excess heat-resistant coating material on the surface of the PET base film to ensure consistent coating thickness. The PET base film coated with the heat-resistant coating material passes through a 15-meter-long oven at a speed of 300 meters / minute to improve the bonding performance of the heat-resistant coating material and the PET base film, wherein the oven temperature is 110°C. During the smoothing process, one of the scraper mechanisms 7 is controlled to operate, and the other scraper mechanism 7 is rotated 90 degrees. After a certain amount of waste material is on the scraper 12, the central axis 11 rotates 90 degrees, and the scraped material can enter the paint collection box 10 from the paint collection inlet 14 for use. The two scraper mechanisms 7 operate in turn, and one is operating while the other is recycling material.

[0072] The heat-resistant coating material prepared in Example 3 was applied to the heat-resistant coating coating process of Example 7. When the thermal transfer carbon ribbon was printed in full black, the effective printing temperature of the carbon ribbon could be increased to 128°C set in the Citizen printer S621C, and there were no defects on the label paper and no cracks on the PET base film. 65 sheets could be printed per minute during continuous printing.

[0073] Example 8: Coating process of heat-resistant coating of thermal transfer carbon ribbon.

[0074] The driving shaft drives the PET base film to move, the carbon belt speed is 310 meters / minute, the coating plate is fixed, and the heat-resistant coating material prepared in Example 3 is uniformly conveyed thereto and uniformly coated on the surface of the PET base film. A smoothing device is used to scrape off the excess heat-resistant coating material on the surface of the PET base film to ensure consistent coating thickness. The PET base film coated with the heat-resistant coating material passes through a 15-meter-long oven at a speed of 310 meters / minute to improve the bonding performance of the heat-resistant coating material and the PET base film, wherein the oven temperature is 115°C. During the smoothing process, one of the scraper mechanisms 7 is controlled to operate, and the other scraper mechanism 7 rotates 90 degrees. After a certain amount of waste material is removed from the scraper 12, the central axis 11 rotates 90 degrees, and the scraped material can enter the paint collection box 10 from the paint collection inlet 14 for use. The two scraper mechanisms 7 operate in turn, and one is operating while the other is recycling material.

[0075] The heat-resistant coating material prepared in Example 4 was applied to the heat-resistant coating coating process of Example 8. When the thermal transfer carbon ribbon was printed in full black, the effective printing temperature of the carbon ribbon could be increased to 128°C set in the Citizen printer S621C, and there were no defects on the label paper and no cracks on the PET base film. 65 sheets could be printed per minute during continuous printing.

[0076] Example 9: Coating process of heat-resistant coating of thermal transfer carbon ribbon.

[0077] The driving shaft drives the PET base film to move, and the carbon belt speed is 295 meters per minute. The coating plate is fixed, and the heat-resistant coating material of the thermal transfer carbon belt prepared in Example 4 is uniformly conveyed thereto and evenly coated on the surface of the PET base film. A smoothing device is used to scrape off the excess heat-resistant coating material on the surface of the PET base film to ensure consistent coating thickness. The PET base film coated with the heat-resistant coating material passes through a 15-meter-long oven at a speed of 300 meters per minute to improve the bonding performance of the heat-resistant coating material and the PET base film, wherein the oven temperature is 115°C. During the smoothing process, one of the scraper mechanisms 7 is controlled to operate, and the other scraper mechanism 7 is rotated 90 degrees. After a certain amount of waste material is removed from the scraper 12, the central axis 11 rotates 90 degrees, and the scraped material can enter the paint collection box 10 from the paint collection inlet 14 for use. The two scraper mechanisms 7 operate in turn, and one recycles the material while the other is operating.

[0078] The heat-resistant coating material prepared in Example 5 was applied to the heat-resistant coating coating process of Example 9. When the thermal transfer carbon ribbon was printed in full black, the effective printing temperature of the carbon ribbon could be increased to 128°C set in the Citizen printer S621C, and there were no defects on the label paper and no cracks on the PET base film. 66 sheets could be printed per minute during continuous printing.

[0079] Example 10: Coating process of heat-resistant coating of thermal transfer carbon ribbon.

[0080] The driving shaft drives the PET base film to move, and the carbon belt speed is 290 meters per minute. The coating plate is fixed, and the heat-resistant coating material of the thermal transfer carbon belt prepared in Example 5 is uniformly conveyed thereto and evenly coated on the surface of the PET base film. A smoothing device is used to scrape off the excess heat-resistant coating material on the surface of the PET base film to ensure consistent coating thickness. The PET base film coated with the heat-resistant coating material passes through a 15-meter-long oven at a speed of 290 meters per minute to improve the bonding performance of the heat-resistant coating material and the PET base film, wherein the oven temperature is 109°C. During the smoothing process, one of the scraper mechanisms 7 is controlled to operate, and the other scraper mechanism 7 is rotated 90 degrees. After a certain amount of waste material is on the scraper 12, the central axis 11 rotates 90 degrees, and the scraped material can enter the paint collection box 10 from the paint collection inlet 14 for use. The two scraper mechanisms 7 operate in turn, and one is operating while the other is recycling material.

[0081] The heat-resistant coating material prepared in Example 1 was applied to the heat-resistant coating coating process of Example 10. When the thermal transfer carbon ribbon was printed in full black, the effective printing temperature of the carbon ribbon could be increased to 128°C set in the Citizen printer S621C, and there were no defects on the label paper and no cracks on the PET base film. 63 sheets could be printed per minute during continuous printing.

[0082] Although the technical solutions of the present invention have been described and listed in detail, it should be understood that it is obvious to those skilled in the art to make modifications to the above embodiments or adopt equivalent alternatives. These modifications or improvements made without departing from the spirit of the present invention are within the scope of protection required by the present invention.

Claims

1. A coating process for a heat-resistant coating of a thermal transfer carbon ribbon, characterized in that: It includes the following steps: Step 1: The driving shaft (1) drives the PET base film (2) to move, the coating plate is fixed, and the heat transfer carbon ribbon heat-resistant coating material is evenly coated on the surface of the PET base film (2), wherein the contents of the heat transfer carbon ribbon heat-resistant coating material are as follows: in parts by weight, 1 to 3 parts of titanium acetylacetonate, 200 to 220 parts of α,ω-dihydroxy polysiloxane with hydroxyl groups as terminal groups, 18 to 22 parts of methacryloxypropyl trimethoxysilane, 2.8 parts of dibutyltin dilaurate, and 7850 to 8850 parts of an organic solvent; Step 2: Use a smoothing device (3) to scrape off excess heat-resistant coating material on the surface of the PET base film (2) to ensure a uniform coating thickness; the smoothing device (3) comprises a device body (5), a smoothing guide roller (6), a scraper mechanism (7) and a flattening roller (8); the smoothing guide roller (6), the scraper mechanism (7) and the flattening roller (8) are all arranged inside the device body (5); a pad (9) is also arranged inside the device body (5); the smoothing guide roller (6) is located in front of the pad (9); the scraper mechanism (7) and the flattening roller (8) are located on the upper side of the pad (9); the flattening roller (8) is located on the rear side of the scraper mechanism (7); the PET base film (2) with the heat-resistant coating passes through the smoothing guide roller (6), between the scraper mechanism (7) and the pad (9), and between the flattening roller (8) and the pad (9) in sequence; the scraper mechanism (7) and the flattening roller (8) pass through the smoothing guide roller (6), between the scraper mechanism (7) and the pad (9), and between the flattening roller (8) and the pad (9); The mechanism (7) is provided with two, the two scraper mechanisms (7) are arranged front and back and operate in turn, the scraper mechanism (7) comprises a paint collection box (10), a central axis (11) and a scraper (12), the front side of the paint collection box (10) is provided with a connecting plate (13), the central axis (11) vertically passes through the connecting plate (13), the front and rear ends of the central axis (11) are connected to the front and rear side walls of the device body (5), the scraper (12) is connected to the lower end of the connecting plate (13), the upper end of the connecting plate (13) and the upper side wall of the paint collection box (10) are between the paint collection inlet (14), the central axis (11) drives the connecting plate (13), the paint collection box (10) and the scraper (12) to rotate under the control of the control device, the scraper (12) is a curved surface structure, and the front side of the connecting plate (13) is a slope structure; Step 3: The drive shaft (1) drives the PET base film (2) coated with the heat-resistant coating material to pass horizontally through a 15-meter-long oven (4) to volatilize the solvent, and the titanium acetylacetonate and the PET base film are , , The active groups undergo a cross-linking reaction to increase the molecular weight, thereby improving the adhesion between the heat-resistant coating material and the PET substrate, and then are transported out through the drive shaft (1).

2. The coating process of the heat-resistant coating of the thermal transfer carbon ribbon according to claim 1, characterized in that: In the step 3, the PET base film (2) after being coated with the heat-resistant coating material moves in the oven (4) at a speed of 290-310 m / min, and a drying temperature of 105-115° C.

3. The coating process of the heat-resistant coating of the thermal transfer carbon ribbon according to claim 1, characterized in that: The organic solvent is one or more of xylene, butanone and cyclohexanone.

4. The coating process of the heat-resistant coating of the thermal transfer carbon ribbon according to claim 1, characterized in that: The method for preparing the heat-resistant coating of the thermal transfer ribbon comprises the following steps: Step 1, weighing titanium acetylacetonate, α,ω-dihydroxy polysiloxane with hydroxyl groups as terminal groups, methacryloxypropyltrimethoxysilane, and an organic solvent, stirring at room temperature for 40 to 60 hours to obtain an organic solution of titanium acetylacetonate; Step 2: Add an organic solvent to the solution obtained in step 1 and stir for 2 to 4 hours; Step 3, weigh dibutyltin dilaurate and add an organic solvent thereto, and stir at room temperature for 15 minutes; Step 4: Add the solution obtained in step 3 to the solution obtained in step 2, and stir for 10 to 20 minutes to obtain the thermal transfer carbon ribbon heat-resistant coating material.