7 series aluminum alloy wire for arc additive manufacturing and its preparation method and application
By optimizing the composition and process of 7-series aluminum alloy wire, combined with extrusion-drawing combined forming and cold metal transition deposition technology, the forming problem of 7-series aluminum alloy wire in arc additive manufacturing has been solved, achieving high strength and The preparation of crack-resistant aluminum alloy wire improves the wire-forming efficiency and component strength.
Patent Information
- Application Number
- CN202211342950.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-31
AI Technical Summary
7 series aluminum alloy wire is difficult to achieve continuous and high-quality wire forming due to severe element burning, sensitive thermal cracking tendency, and difficulty in processing and forming during arc additive manufacturing. Moreover, the heat input of traditional gas metal arc welding is large. Resulting in poor forming and reduced strength.
By optimizing the content of elements such as Zn, Mg, and Cu, using micro-alloying treatments such as Ti, Zr, and Sc, combined with extrusion-drawing combined forming technology and cold metal transition deposition methods, the composition and process parameters are designed to obtain high strength and resistance. 7 series aluminum alloy wire with excellent cracking performance.
The 7-series aluminum alloy wire that achieves ultra-high strength and good crack resistance solves the cracking problem, improves the wire-forming efficiency and yield rate, reduces production costs, and obtains high-strength aluminum alloy by optimizing the deposition process parameters. member.
Smart Images

Figure CN116144993B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of aluminum alloy forming, and in particular relates to a 7 series aluminum alloy wire for arc additive manufacturing, and a preparation method and application thereof. Background Art
[0002] Aluminum alloy arc fuse additive manufacturing technology is highly efficient and low-cost, has significant advantages in the manufacture of large flexible structures, and has broad application prospects in the aerospace field. Since 2-series, 4-series, 5-series and 6-series aluminum alloys have low strength, high plasticity, and good wire drawing properties, the forming technology for the above wires is already very mature and has been commercialized. At present, aluminum alloy parts manufactured by arc fuse additive manufacturing using the above wires have been successfully used in aerospace, weapons and equipment, and rail transportation.
[0003] With the increasing demand for lightweight structures and high-strength aluminum alloys, the demand for 7-series ultra-high-strength aluminum alloy arc fuse additive manufacturing technology is becoming more and more urgent. At present, there are relatively many studies on 7-series aluminum alloy powder laser additive manufacturing, and the use of various types of 7-series aluminum alloys for additive manufacturing has been initially realized through laser selective deposition. However, the research and application of arc additive manufacturing for 7-series aluminum alloy wires is still in its infancy. This is mainly restricted by the metallurgical properties and processing technology of 7 series aluminum alloy wire: (1) 7 series aluminum alloy contains more alloying elements such as Zn, Mg, and Cu. During the arc additive manufacturing process, the element burnout is more serious and the tendency of thermal cracking is very sensitive, making it difficult to achieve a continuous arc additive manufacturing process; (2) The work hardening and precipitation strengthening effects of 7 series aluminum alloy are strong. It is very easy to crack during wire extrusion, rolling, and wire drawing. As a result, it is difficult to continuously and stably obtain high-quality 7 series aluminum alloy wire using conventional aluminum alloy wire forming processes; (3) Due to the large heat input of traditional metal arc welding, the wall is easy to collapse during the additive process, the surface forming is poor, and the grain growth tendency of the deposit is large, which significantly reduces the strength. Therefore, the composition design, forming processing technology, and additive manufacturing method of 7 series aluminum alloy wire are the key issues restricting the application of 7 series aluminum alloy in the field of arc fuse additive manufacturing. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention proposes a 7 series aluminum alloy wire for arc additive manufacturing, a preparation method and an application thereof, so as to obtain ultra-high strength 7 series aluminum alloy wire for arc additive manufacturing, that is, by optimizing the content of main alloying elements Zn, Mg and Cu, utilizing micro-alloying treatment of elements such as Ti, Zr and Sc, and controlling the content of impurity elements Fe, Si and H, while ensuring ultra-high strength, it also has good thermal cracking resistance; by designing and using extrusion dies and improving extrusion technology, the extrusion-wire drawing combined forming technology is utilized to realize efficient short-process processing and production of 7 series aluminum alloy wire; by adopting the cold metal transition (CMT) stacking method, by optimizing the stacking process parameters, aluminum alloy components that meet the strength performance requirements are produced, and the cracking problem of existing additive aluminum alloy components is solved.
[0005] The first technical problem solved by the present invention is to provide a 7-series aluminum alloy wire composition for arc additive manufacturing that can achieve ultra-high strength and good crack resistance;
[0006] The second technical problem to be solved by the present invention is to provide a forming and processing technology capable of realizing short-process high-quality production of 7 series aluminum alloy wire for arc additive manufacturing, that is, a preparation method thereof;
[0007] The third technical problem to be solved by the present invention is to provide an arc additive manufacturing method using 7 series aluminum alloy wire for arc additive manufacturing to achieve ultra-high strength requirements.
[0008] The technical solution adopted by the present invention to solve the above-mentioned first technical problem is: a 7 series aluminum alloy wire for arc additive manufacturing, whose design composition (mass percentage wt.%) is shown in Table 1. Design basis: Zn, Mg and Cu are the main strengthening elements in the 7 series aluminum alloy wire for arc additive manufacturing. (1) When the Zn content is too high and exceeds the solid solubility of Zn in the aluminum matrix, on the one hand, the strengthening effect of Zn cannot continue to increase, and on the other hand, serious Zn element evaporation will occur during arc additive manufacturing; when the Zn content is too low, the strengthening effect of Zn cannot meet the strength requirements of the aluminum alloy. Therefore, the Zn content is controlled between 6.0-10.0%. (2) In the 7 series aluminum alloy wire for arc additive manufacturing, the Zn / Mg ratio is generally required to be between 3.2-3.6, which is conducive to the precipitation of η (MgZn2) strengthening phase and improves the strength of the aluminum alloy, so the Mg content is controlled between 1.5-2.8%. (3) In the 7 series aluminum alloy wire for arc additive manufacturing, the Cu element mainly improves the strength of the aluminum alloy by forming S (Al2CuMg) phase and θ (Al2Cu) phase. When the Cu content is too high, the crack resistance of the aluminum alloy is reduced. When it is too low, the strength requirements of the aluminum alloy cannot be met. Therefore, the Cu content is controlled between 1.0-2.2%. (4) The addition amount of Ti, Zr, and Sc is based on the solid solubility of the three elements in the aluminum alloy matrix on the one hand, and on the other hand, the effect of the three elements on refining the grain structure of the aluminum alloy is comprehensively considered.
[0009] Table 1 Composition design range of 7 series aluminum alloy wire for arc additive manufacturing (wt.%)
[0010]
[0011] The technical solution adopted by the present invention to solve the above second technical problem is: a method for preparing a 7 series aluminum alloy wire for arc additive manufacturing, which is processed into an aluminum alloy wire with a diameter of 1.2 mm by extrusion-wire drawing combined forming technology, comprising the following steps:
[0012] Step 1: Prepare the ingredients according to the designed composition of the 7 series aluminum alloy wire for arc additive manufacturing, where Cu, Ti, Zr, and Sc are added in the form of master alloys, and Zn and Mg are added in the form of pure metals. First, melt the pure aluminum ingot, then add the Cu, Ti, Zr, and Sc master alloys, and finally add Zn and Mg pure metals after all are melted to obtain an alloy melt.
[0013] Step 2: Sampling and analysis. After all chemical components in the alloy melt are qualified, semi-continuous casting begins. The casting temperature is 750-780°C, the billet drawing speed is 50-70mm / min, and the cooling water flow rate is 60-100L / min to obtain an ingot. Subsequently, the ingot is subjected to homogenization heat treatment at a heat treatment temperature of 460-480°C and a holding time of 24-36h, and then air-cooled out of the furnace.
[0014] Step 3: Saw the heat-treated ingot into segments, peel it, and put it into the extruder for extrusion processing. The first extrusion is to extrude a rod with a diameter of 9.5 mm. The extrusion die heating temperature is 380-420°C, the ingot preheating temperature is 380-410°C, and the extrusion speed is 0.5-1.0 mm / s; the second extrusion is to extrude a wire with a diameter of 2.7 mm at an extrusion speed of 1.0-3.0 mm / s.
[0015] Step 4: After multiple annealing and wire drawing, mechanical scraping, ultrasonic cleaning, and passivation treatments, the wire with a diameter of 2.7 mm is processed into a finished wire with a diameter of 1.2 mm.
[0016] The technical solution adopted by the present invention to solve the above-mentioned third technical problem is: adopting the cold metal transition (CMT) stacking method, using the designed 7 series aluminum alloy wire as the filling material for arc additive manufacturing, through experimental research and optimization, adopting the following stacking process parameters: current 90~160A, voltage 9.8~12.5V, stacking speed 450~620mm / min, protective gas (argon with a purity of 99.99%) flow rate 18~25L / min, the aluminum alloy deposit can obtain a fine equiaxed crystal structure and achieve the high strength and good crack resistance of the 7 series aluminum alloy wire.
[0017] The beneficial effects of the present invention are:
[0018] 1. In the composition design of the present invention, the content of Zn and Mg elements is appropriately increased to compensate for the burning loss of the elements in the subsequent arc additive manufacturing process and ensure the strength of the components after additive manufacturing; micro-alloying elements such as Ti, Zr, Sc are jointly added to refine the grain structure of the aluminum alloy components manufactured by arc additive manufacturing and improve the crack resistance of the aluminum alloy components in the additive manufacturing process; adding Ti and Zr elements to replace part of the Sc element can significantly reduce the cost of aluminum alloy wire.
[0019] 2. The present invention proposes an aluminum alloy wire forming technology through two extrusions (the first extrusion is a rod with a diameter of 9.5 mm, and the second extrusion is a wire with a diameter of 2.7 mm) and multiple wire drawing (processed into a wire with a diameter of 1.2 mm). Compared with the conventional aluminum alloy wire forming technology of processing a rod with a diameter of about 9.5 mm into a finished wire with a diameter of 1.2 mm through multiple wire drawing, this forming technology fundamentally solves the cracking and wire breaking phenomenon caused by the extremely low plasticity of the aluminum alloy caused by its extremely strong work hardening and precipitation strengthening during the rolling and wire drawing process of the 7 series aluminum alloy wire, greatly improving the wire forming efficiency and yield rate in the preparation process of the 7 series ultra-high strength aluminum alloy wire, and effectively reducing the production cost.
[0020] 3. The 7 series aluminum alloy wire of the present invention adopts the cold metal transition (CMT) deposition method, and achieves the ultra-high strength of the arc-added aluminum alloy component by optimizing the deposition process parameters. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The metallographic structure diagram of the aluminum alloy deposit prepared in Example 1;
[0022] Figure 2 This is the metallographic structure diagram of the aluminum alloy deposit prepared in Example 2. DETAILED DESCRIPTION
[0023] In order to better explain the present invention and facilitate understanding, the technical solutions and effects of the present invention are described in detail below through specific implementation methods.
[0024] Embodiment 1:
[0025] The chemical composition (mass percentage) of the designed 7 series aluminum alloy wire is: Zn 7.6%, Cu 1.8%, Mg 2.2%, Ti 0.16%, Zr 0.22%, Sc 0.25%, Si 0.05%, Fe 0.10%, and the rest is Al.
[0026] High-strength aluminum alloy wire smelting and forming processing technology:
[0027] Step 1: Prepare the ingredients according to the designed composition of the wire material. First, melt the pure aluminum ingot, then add the intermediate alloys such as Cu, Ti, Zr, Sc, etc., and finally add the pure metals Zn and Mg after all are melted to obtain the alloy melt.
[0028] Step 2: Sampling and analysis. After all chemical components in the alloy melt are qualified, semi-continuous casting begins. The casting temperature is 750℃, the billet drawing speed is 50mm / min, and the cooling water flow rate is 70L / min to obtain an ingot. Subsequently, the ingot is subjected to homogenization heat treatment at a heat treatment temperature of 470℃ and a holding time of 24h, and then air-cooled out of the furnace.
[0029] Step 3: Saw the heat-treated ingot into segments, peel it, and put it into the extruder for extrusion processing. The first extrusion is extruded into a rod with a diameter of 9.5mm. The extrusion die heating temperature is 400℃, the ingot preheating temperature is 390℃, and the extrusion speed is 0.8mm / s; the second extrusion is extruded into a wire with a diameter of 2.7mm, and the extrusion speed is 2.5mm / s.
[0030] Step 4: After multiple annealing and wire drawing, mechanical scraping, ultrasonic cleaning, and passivation treatment, the wire with a diameter of 2.7 mm is processed into a finished wire with a diameter of 1.2 mm.
[0031] Using the 7 series aluminum alloy wire with the above composition, arc additive manufacturing was carried out by cold metal transfer (CMT) deposition method. The deposition process parameters are as follows: current 110A, voltage 11.8V, deposition speed 540mm / min, shielding gas (argon) flow rate 18L / min. The obtained aluminum alloy deposit is mainly composed of fine equiaxed crystals, such as Figure 1 As shown, the mechanical properties of the pile in the horizontal direction are as follows: tensile strength is 367MPa, yield strength is 311MPa, and elongation is 4.3%; after T6 heat treatment, the mechanical properties are improved to: tensile strength is 634MPa, yield strength is 535MPa, and elongation is 5.7%.
[0032] Embodiment 2:
[0033] The composition (mass fraction) of the designed 7 series aluminum alloy wire is: Zn 8.2%, Cu 1.5%, Mg 1.8%, Ti 0.20%, Zr 0.18%, Sc 0.22%, Si 0.06%, Fe 0.09%, and the rest is Al.
[0034] High-strength aluminum alloy wire smelting and forming processing technology:
[0035] Step 1: Prepare the ingredients according to the designed composition of the wire material. First, melt the pure aluminum ingot, then add the intermediate alloys such as Cu, Ti, Zr, Sc, etc., and finally add the pure metals Zn and Mg after all are melted to obtain the alloy melt.
[0036] Step 2: Sampling and analysis. After all the chemical compositions of the alloy are qualified, semi-continuous casting begins. The casting temperature is 780℃, the billet drawing speed is 60mm / min, and the cooling water flow rate is 80L / min to obtain an ingot. Subsequently, the ingot is subjected to homogenization heat treatment at a temperature of 480℃ and a holding time of 30h, and then air-cooled after being taken out of the furnace.
[0037] Step 3: Saw the heat-treated ingot into segments, peel it, and put it into the extruder for extrusion processing. The first extrusion is extruded into a rod with a diameter of 9.5mm. The extrusion die heating temperature is 420℃, the ingot preheating temperature is 410℃, and the extrusion speed is 0.5mm / s; the second extrusion is extruded into a wire with a diameter of 2.7mm, and the extrusion speed is 1.8mm / s.
[0038] Step 4: After multiple annealing and wire drawing, mechanical scraping, ultrasonic cleaning, and passivation treatments, the wire with a diameter of 2.7 mm is processed into a finished product with a diameter of 1.2 mm.
[0039] Using the 7 series aluminum alloy wire with the above composition, arc additive manufacturing was carried out by cold metal transfer (CMT) deposition method. The deposition process parameters are as follows: current 120A, voltage 12.2V, deposition speed 620mm / min, shielding gas (argon) flow rate 25L / min. The obtained aluminum alloy wire deposition body is mainly composed of fine equiaxed crystals, such as Figure 2 As shown, the mechanical properties of the pile in the horizontal direction are as follows: tensile strength is 358MPa, yield strength is 302MPa, and elongation is 4.8%; after T6 heat treatment, the mechanical properties are improved to: tensile strength is 622MPa, yield strength is 521MPa, and elongation is 6.2%.
Claims
1. A method for preparing 7 series aluminum alloy wire for arc additive manufacturing, characterized in that: The composition of 7 series aluminum alloy wire for arc additive manufacturing includes Zn, Mg, Cu, Ti, Zr, Sc, Fe, Si, and Al; The composition and mass percentage of the 7 series aluminum alloy wire for arc additive manufacturing are respectively Zn 6.0-10.0%, Mg 1.5-2.8%, Cu 1.0-2.2%, Ti 0.16-0.25%, Zr 0.18-0.25%, Sc 0.10-0.45%, Fe≤0.15%, Si≤0.10%, and the rest is Al; The preparation method comprises the following steps: Step 1: The ingredients are prepared according to the designed composition of the 7 series aluminum alloy wire for arc additive manufacturing, wherein Cu, Ti, Zr, and Sc are added in the form of master alloys, and Zn and Mg are added in the form of pure metals; first, the pure aluminum ingot is melted, and then the Cu, Ti, Zr, and Sc master alloys are added. After all the master alloys are melted, Zn and Mg pure metals are finally added to obtain an alloy melt; Step 2: Sampling and analysis. After all chemical components in the alloy melt are qualified, semi-continuous casting begins; the casting temperature is 750-780 °C, the billet drawing speed is 50-70 mm / min, and the cooling water flow rate is 60-100 L / min to obtain an ingot; then, the ingot is subjected to homogenization heat treatment at a heat treatment temperature of 460-480 °C, a holding time of 24-36 hours, and air cooling after being taken out of the furnace; Step 3: saw the heat-treated ingot into segments, peel it, and put it into the extruder for extrusion processing; the first extrusion is to extrude a rod with a diameter of 9.5 mm; the extrusion die heating temperature is 380~420℃, the ingot preheating temperature is 380~410℃, and the extrusion speed is 0.5~1.0mm / s; the second extrusion is to extrude a wire with a diameter of 2.7 mm, and the extrusion speed is 1.0~3.0mm / s; Step 4: After multiple annealing and wire drawing, mechanical scraping, ultrasonic cleaning, and passivation treatments, the wire with a diameter of 2.7 mm is processed into a finished wire with a diameter of 1.2 mm.
2. Application of the 7 series aluminum alloy wire for arc additive manufacturing prepared by the method according to claim 1, characterized in that: The arc additive manufacturing method of the 7 series aluminum alloy wire is as follows: adopting a cold metal transition deposition method, using the designed 7 series aluminum alloy wire as a filling material to perform arc additive manufacturing, and obtaining an aluminum alloy deposit with a fine equiaxed crystal structure; The deposition process parameters adopted are: current 90~160A, voltage 9.8~12.5V, deposition speed 450~620mm / min, and protective gas flow rate 18~25L / min.
3. The use of the 7 series aluminum alloy wire for arc additive manufacturing according to claim 2, characterized in that: The protective gas is argon with a purity of 99.99%.
Citation Information
Patent Citations
Al-Zn-Mg-Sc series aluminum alloy wire for 3D printing and preparation method thereof
CN111471905A
Aluminum alloy additive manufacturing method assisted by stirring friction machining
CN114147340A