Aluminum alloy-inorganic titanium ceramic-graphene composite material and preparation method thereof
Through the preparation method of aluminum alloy-inorganic titanium porcelain-graphene composite materials, the problems of graphene heating film that is not resistant to high temperatures, has no hardness, and is easy to deform are solved, achieving high hardness, fire resistance and rapid heat dissipation, and improving the material quality. comprehensive performance and security.
Patent Information
- Application Number
- CN202211549581.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Existing graphene heating films are not resistant to high temperatures, have no hardness, are easily deformed, are flammable, and have problems with poor bonding force and potential safety hazards.
The preparation method of aluminum alloy-inorganic titanium porcelain-graphene composite material is adopted, and the aluminum alloy-inorganic titanium porcelain- Graphene film composite material enhances bonding strength and high temperature resistance.
It achieves high hardness, Class A fire protection, high temperature resistance of 1200°C, resistance to deformation and rapid heat dissipation, improving the overall performance and safety of the material.
Smart Images

Figure BDA0003980488300000071
Abstract
Description
Technical Field
[0001] The present invention relates to the field of graphene heating films, and in particular to an aluminum alloy-inorganic titanium ceramic-graphene composite material and a preparation method thereof. Background Art
[0002] Graphene heating film is one of the emerging heating methods. It is a structure that uses electric energy as a source and releases far-infrared radiation through graphene for heat transfer. It has excellent properties such as uniform heating, fast temperature rise, and electric heat conversion efficiency of up to 99.5%, so it has been widely used. Graphene has extremely high thermal conductivity and thermal radiation coefficient. The thermal conductivity of a single layer of graphene is as high as 5300W / mK, which is much higher than the highest thermal conductivity of metals such as gold, silver, copper, and aluminum, and has good flexibility. The 8-14μm far infrared rays generated during the working process of the graphene heating film are the most suitable band for human health, which can promote blood circulation and improve the body's immune ability. Graphene also has high strength and ultra-large specific surface area, making graphene one of the most attractive materials in the field of electric heating film. However, at present, the industrialized graphene heating film generally adopts chemical vapor deposition (CVD) with PVC film as the carrier, but this product has the disadvantages of not being resistant to high temperature (easy to burn at about 200℃), no hardness, easy to deform, and flammable.
[0003] A multi-layer fast-heating electric heater containing graphene and aluminum alloy (application number: 201810085791.0), including a controller, a bracket, a hollow square frame and a multi-layer heating mechanism; the multi-layer heating mechanism includes, from front to back, an aluminum alloy front plate, a first insulating layer, a first graphene heating film, a second insulating layer, a first heat-reflecting thermal insulation layer, a cavity, a second graphene heating film, a third insulating layer, a second heat-reflecting thermal insulation layer and a back plate, and a plurality of ventilation micropores are provided on the aluminum alloy front plate. However, the aluminum alloy front plate, the first insulating layer and the first graphene heating film are physically bonded, and the bonding force is poor. After long-term high-temperature use, cracks are easily generated between the layers. In addition, the insulating layer is easily deformed and flammable under long-term high temperatures, which poses a safety hazard. Summary of the invention
[0004] In view of the problems existing in the prior art such as the graphene heating film being not resistant to high temperatures, having no hardness, being easy to deform and being flammable, the purpose of the present invention is to provide an aluminum alloy-inorganic titanium ceramic-graphene composite material and a preparation method thereof.
[0005] The purpose of the present invention is achieved by the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing an aluminum alloy-inorganic titanium ceramic-graphene composite material, comprising the following steps:
[0007] (1) Soak the aluminum alloy in a diluted degreasing / etching agent at room temperature until the surface water film is completely spread and corrosion white appears;
[0008] (2) washing the aluminum alloy treated in step (1), drying it, and setting it aside;
[0009] (3) applying the inorganic titanium ceramic coating on the surface of the aluminum alloy obtained in step (2), and then drying it to form an aluminum alloy-inorganic titanium ceramic coating composite material for standby use;
[0010] (4) treating the aluminum alloy-inorganic titanium ceramic coating composite material obtained in step (3) at high temperature, and then applying the dispersed graphene infiltration liquid on the surface to form an aluminum alloy-inorganic titanium ceramic coating-graphene film composite material for standby use;
[0011] (5) An inorganic titanium ceramic coating is attached to the surface of the aluminum alloy-inorganic titanium ceramic coating-graphene film composite material obtained in step (4) and dried to complete the preparation.
[0012] Preferably, in step (1), the degreasing / etching agent comprises the following components calculated by mass fraction:
[0013] 10% to 20% potassium hydroxide, 5% to 10% anhydrous sodium metasilicate, 1% to 5% sodium gluconate, 1% to 5% disodium ethylenediaminetetraacetate, 5% to 10% fatty alcohol polyether (HLB is 11 to 13), and the balance is water.
[0014] Preferably, in step (1), the dilution is to dilute the degreasing / etching agent by 10 to 20 times, so as to remove oil stains, dust, etc. on the surface and to etch the surface to a certain extent.
[0015] Preferably, in step (1), the soaking time is 5 to 15 minutes.
[0016] Preferably, in step (1), the amount of aluminum alloy etched is greater than 2.0 g / m 2 .
[0017] Preferably, in step (2), the drying is to air-dry the sample or to bake it at 80-100°C.
[0018] Preferably, in step (3), the inorganic titanium ceramic coating comprises the following components calculated by mass fraction:
[0019] 0.5% to 2% silicon dioxide, 0.5% to 2% titanium dioxide, 2% to 4% aluminum oxide fiber, 0.5% to 2% cerium oxide, 0.2% to 0.5% inorganic vitrified microspheres, 1% to 2% attapulgite, and the balance is solvent.
[0020] The solvent is a PVA solution with a mass fraction of 1%, and the solvent is referenced to the zirconia ceramic coating.
[0021] Preferably, the aspect ratio of the aluminum oxide fiber is 8-15.
[0022] Preferably, in step (3), the thickness of the inorganic titanium ceramic coating layer is 15 to 30 μm.
[0023] Preferably, in step (3), the drying is performed naturally for 24 hours.
[0024] Preferably, in step (4), the temperature of the high temperature treatment is 850°C.
[0025] Preferably, in step (4), the graphene permeate solution comprises graphene powder and nano bamboo charcoal powder. The mass ratio of graphene powder to nano bamboo charcoal powder is 1:3, and this ratio is based on the graphene oxide pervaporation membrane, and 0.1g of graphene oxide and 0.3g of chitosan are added to a 2wt% acetic acid solution.
[0026] Preferably, in step (4), the graphene infiltration liquid needs to be acidified, and the process of the acidification treatment is as follows: concentrated sulfuric acid and fuming nitric acid are mixed in a mass ratio of 1:2, expandable graphite is placed in the solution and magnetically stirred to obtain a graphene oxide solution, the graphene oxide is concentrated and adjusted to a concentration of 10 mg / ml, and then the graphene oxide solution is coated on a substrate treated with a surface active agent, and dried for 24 hours to obtain a graphene oxide film, which is then reduced at 80°C in an atmosphere of hydroiodic acid and pressed to obtain a graphene high thermal conductivity film.
[0027] Preferably, in step (4), the thickness of the graphene film layer is 0.1 mm to 0.2 mm.
[0028] Preferably, in step (5), the drying is natural drying for 24 hours.
[0029] In a second aspect, the present invention provides an aluminum alloy-inorganic titanium ceramic-graphene composite material prepared using the above-mentioned preparation method.
[0030] In a third aspect, the present invention provides an application of an aluminum alloy-inorganic titanium ceramic-graphene composite material prepared by the above-mentioned preparation method in the fields of medical equipment, civilian household appliances, and health and physiotherapy.
[0031] The beneficial effects of the present invention are:
[0032] 1. Compared with the prior art, the present invention forms a high-hardness heating film through a three-layer composite of aluminum alloy, inorganic titanium ceramic coating and graphene. It has good bonding force, Class A fireproof, and can withstand high temperatures of 1200°C; the hardness is 4H~9H, it is not easy to deform at high temperatures, and has fast heat dissipation.
[0033] 2. The inorganic titanium ceramic coating of the present invention can not only solve the bonding problem between aluminum alloy and graphene, but also improve the hardness and high temperature resistance, and also has a fireproof function.
[0034] 3. The composition of inorganic titanium ceramic coating contains aluminum oxide fiber material, inorganic glass microspheres and attapulgite. Among them, aluminum oxide fiber materials overlap and connect to form a high-speed heat dissipation channel, and are distributed in a three-dimensional network in the entire insulating rubber layer. The three-dimensional structure formed by aluminum oxide fibers is also conducive to improving the bonding between the inorganic titanium ceramic coating and the aluminum alloy and graphene layer. Titanium ceramic coating is a pure inorganic coating with low surface requirements. As long as the surface has a certain degree of roughness, no oil stains and oxide scale, it has good adhesion. Among them, inorganic glass microspheres are an acidic glassy lava mineral. After special technical treatments such as high-temperature expansion in a gas furnace and production process processing, they are formed into spherical fine-diameter particles with porous interior, glassy and closed surface, stable physical and chemical properties, and Class A combustion performance. It is an environmentally friendly inorganic lightweight insulation material. Since the surface of the expanded vitrified microspheres is vitrified to form a certain particle strength, the physical and chemical properties are very stable, the aging and weather resistance are strong, and they have excellent insulation and fire resistance. They are suitable for use as lightweight filling aggregates in many fields, and can also reduce material shrinkage, improve product comprehensive performance, and reduce comprehensive production costs. High-temperature resistant attapulgite has unique dispersion, high temperature resistance, salt and alkali resistance and other good colloidal properties and high adsorption and decolorization ability, plasticity and adhesion. DETAILED DESCRIPTION
[0035] In order to more clearly illustrate the present invention and have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0036] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0037] The present invention is further described in conjunction with the following examples.
[0038] Example 1
[0039] A preparation method of an aluminum alloy-inorganic titanium ceramic-graphene composite material mainly comprises the following steps:
[0040] (1) Soak the aluminum alloy in the diluted degreasing / etching agent at room temperature for 5 minutes until the surface water film is completely spread and corrosion white appears; the aluminum alloy etching amount is greater than 2.0g / m 2 ;
[0041] (2) washing the aluminum alloy treated in step (1) with water, and then drying the sample for later use;
[0042] (3) applying the inorganic titanium ceramic coating to the surface of the aluminum alloy obtained in step (2), and then naturally drying for 24 hours to form an aluminum alloy-inorganic titanium ceramic coating composite material for standby use;
[0043] (4) heating the aluminum alloy-inorganic titanium ceramic coating composite material obtained in step (3) to 850° C., and then applying the dispersed graphene infiltration liquid on the surface to form an aluminum alloy-inorganic titanium ceramic coating-graphene film composite material for standby use;
[0044] (5) An inorganic titanium ceramic coating is attached to the surface of the aluminum alloy-inorganic titanium ceramic coating-graphene film composite material obtained in step (4), and the mixture is naturally dried for 24 hours to complete.
[0045] The degreasing / etching agent includes the following components and their mass fractions: 10% potassium hydroxide, 5% anhydrous sodium metasilicate, 1% sodium gluconate, 1% disodium ethylenediaminetetraacetate, 5% fatty alcohol polyether HLB11-13, and the balance water. Dilute 10 times before use, at room temperature, for 15 minutes, to remove surface oil, dust, etc., and at the same time form a certain etching on the surface.
[0046] The inorganic titanium ceramic coating includes the following components and their mass fractions: 0.5% silicon dioxide, 0.5% titanium dioxide, 2% aluminum oxide fiber, 0.5% cerium oxide, 0.2% inorganic vitrified microspheres, 1% attapulgite, and the remainder of solvent. The aspect ratio of the aluminum oxide fiber is 8 to 15. The graphene infiltration liquid includes graphene powder and nano bamboo charcoal powder. The graphene infiltration liquid is acidified.
[0047] Example 2
[0048] A preparation method of an aluminum alloy-inorganic titanium ceramic-graphene composite material mainly comprises the following steps:
[0049] (1) Soak the aluminum alloy in the diluted degreasing / etching agent at room temperature for 15 minutes until the surface water film is completely spread and corrosion white appears; the aluminum alloy etching amount is greater than 2.0g / m 2 ;
[0050] (2) washing the aluminum alloy treated in step (1) with water, and then drying the sample at 80-100° C. for later use;
[0051] (3) applying the inorganic titanium ceramic coating to the surface of the aluminum alloy obtained in step (2), and then naturally drying for 24 hours to form an aluminum alloy-inorganic titanium ceramic coating composite material for standby use;
[0052] (4) heating the aluminum alloy-inorganic titanium ceramic coating composite material obtained in step (3) to 850° C., and then applying the dispersed graphene infiltration liquid on the surface to form an aluminum alloy-inorganic titanium ceramic coating-graphene film composite material for standby use;
[0053] (5) An inorganic titanium ceramic coating is attached to the surface of the aluminum alloy-inorganic titanium ceramic coating-graphene film composite material obtained in step (4), and the mixture is naturally dried for 24 hours to complete.
[0054] The degreasing / etching agent includes the following components and their mass fractions: 20% potassium hydroxide, 10% anhydrous sodium metasilicate, 5% sodium gluconate, 5% disodium ethylenediaminetetraacetate, 10% fatty alcohol polyether HLB11-13, and the balance water. Dilute 20 times before use, at room temperature, process for 5 minutes, remove surface oil, dust, etc., and at the same time form a certain etching on the surface.
[0055] The inorganic titanium ceramic coating includes the following components and their mass fractions: 2% silicon dioxide, 2% titanium dioxide, 4% aluminum oxide fiber, 2% cerium oxide, 0.5% inorganic vitrified microspheres, 2% attapulgite, and the remainder of solvent. The aspect ratio of the aluminum oxide fiber is 8 to 15. The graphene infiltration liquid includes graphene powder and nano bamboo charcoal powder. The graphene infiltration liquid is acidified.
[0056] Comparative Example 1
[0057] A preparation method of an aluminum alloy-titanium dioxide-graphene heating composite material mainly includes the following steps:
[0058] (1) Soak the aluminum alloy in the diluted degreasing / etching agent at room temperature for 5 to 15 minutes until the surface water film is completely spread and corrosion white appears;
[0059] (2) washing the aluminum alloy treated in step (1) with water, and then air-drying the sample or drying it at 80-100° C. for later use;
[0060] (3) coating titanium dioxide on the surface of the aluminum alloy obtained in step (2), and then naturally drying it for 24 hours to form an aluminum alloy-titanium dioxide composite material for later use;
[0061] (4) heating the aluminum alloy-titanium dioxide composite material obtained in step (3) to 850° C., and then applying the dispersed graphene infiltration liquid on the surface to form an aluminum alloy-titanium dioxide-graphene film composite material for standby use;
[0062] (5) applying electrophoretic paint to the surface of the aluminum alloy-titanium dioxide-graphene film composite material obtained in step (4).
[0063] The degreasing / etching agent includes the following components and their mass fractions: potassium hydroxide 20%, anhydrous sodium metasilicate 10%, sodium gluconate 5%, disodium ethylenediaminetetraacetic acid 5%, fatty alcohol polyether HLB11-13 10%, and the balance water. Dilute 20 times before use, at room temperature, treat for 5 minutes, remove surface oil, dust, etc., and form a certain etching on the surface. The graphene penetration liquid includes graphene powder and nano bamboo charcoal powder. The graphene penetration liquid is acidified.
[0064] Comparative Example 2
[0065] The preparation method is the same as that of Example 1, except that the degreasing / etching agent of Example 1 is replaced with an aluminum alloy degreasing cleaning agent, which includes 7 to 14 parts of ethanol, 15 to 25 parts of water-soluble phosphate, 6 to 10 parts of sodium bicarbonate, 6 to 10 parts of sodium molybdate, 2 to 7 parts of magnesium hydroxide, 1 to 5 parts of sodium dodecyl sulfate and 33 to 59 parts of water. The adhesion becomes worse and becomes level 1.
[0066] Comparative Example 3
[0067] The preparation method is the same as that of Example 1, except that the aluminum oxide fibers in the inorganic titanium ceramic coating are replaced with aluminum oxide nanoparticles. The adhesion is deteriorated to level 1, the heat dissipation is deteriorated, the volume resistivity is 0.004-0.015Ω·m, and the surface resistivity is 0.4-2Ω / sq.
[0068] Comparative Example 4
[0069] The preparation method is the same as that of Example 1, except that the inorganic titanium ceramic coating does not contain inorganic vitrified microspheres and attapulgite. The hardness is 8H; the adhesion is also deteriorated to level 1. The high temperature resistance is reduced, and the high temperature resistance can be 900°C.
[0070] Comparative Example 5
[0071] The preparation method is the same as that of Example 1, except that the inorganic titanium ceramic coating is attached to the surface of the obtained aluminum alloy-inorganic titanium ceramic coating-graphene film layer composite material in step (5) is replaced by electrophoretic paint attached to the surface of the obtained aluminum alloy-inorganic titanium ceramic coating-graphene film layer composite material. The high temperature resistance is reduced and can withstand a high temperature of 1100°C.
[0072] Experimental example
[0073] (1) Test results of the aluminum alloy-inorganic titanium ceramic-graphene composite materials obtained in Example 1 and Example 2:
[0074] The surface density of the aluminum alloy-inorganic titanium ceramic-graphene composite material obtained in Example 1 is 25-40 g / m 3The volume resistivity is 0.001~0.01Ω·m, and the surface resistivity is 0.2~1Ω / sq.
[0075] The aluminum alloy-inorganic titanium ceramic-graphene composite materials obtained in Example 1 and Example 2 were placed in a muffle furnace at a temperature of 400° C. for 2 hours, and there was no shedding, cracking or bending between the layers.
[0076] The aluminum alloy-inorganic titanium ceramic-graphene composite materials obtained in Example 1 and Example 2 were placed in a muffle furnace at a temperature of 1200° C. for 10 to 20 seconds, and there was no shedding, cracking or bending between the layers. They were not easily deformed at high temperatures.
[0077] (2) Test results of the aluminum alloy-titanium dioxide-graphene heating composite material obtained in Comparative Example 1:
[0078] The surface density of the aluminum alloy-titanium dioxide-graphene heating composite material obtained in Comparative Example 1 is 10-35 g / m 3 , volume resistivity is 0.005~0.02Ω·m, surface resistivity is 0.7~3Ω / sq. Class A fireproof, high temperature resistance 700℃; hardness is 6H, adhesion is also poor, becoming Class 1.
[0079] The aluminum alloy-titanium dioxide-graphene heating composite material obtained in Comparative Example 1 was placed in a muffle furnace at a temperature of 300°C for 2 hours, and there was no shedding, cracking, or bending between the layers. At 350°C, it was placed for 2 hours, and cracks and bending began to appear between the layers.
[0080] The aluminum alloy-titanium dioxide-graphene heating composite material of comparative example 1 was placed in a muffle furnace. When the temperature was 700°C and placed for 10 to 20 seconds, there was no shedding, cracking or bending between the layers. When the temperature was 750°C and placed for 10 to 20 seconds, cracks and bending appeared between the layers. When the temperature was 800°C, some of the layers fell off.
[0081] (3) The aluminum alloy-inorganic titanium ceramic-graphene composite material obtained in Example 1 was tested, and the thickness of the inorganic titanium ceramic coating layer was 15 to 30 microns; the thickness of the graphene film layer was 0.1 mm to 0.2 mm. It was Class A fireproof and could withstand high temperatures of 1200°C; and the hardness was 9H.
[0082] The test data is shown in Table 1.
[0083] Table 1 Test data of Example 1
[0084]
[0085]
[0086] It can be seen from the above tests that the aluminum alloy-inorganic titanium ceramic-graphene composite material prepared by the present invention has good bonding strength, fire resistance, and high temperature resistance; it has the advantages of high hardness, not easy to deform at high temperature, and fast heat dissipation.
[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing an aluminum alloy-inorganic titanium ceramic-graphene composite material, characterized in that: The following steps are involved: (1) Soak the aluminum alloy in a diluted degreasing / etching agent at room temperature until the surface water film is completely spread out and corrosion white appears; (2) washing and drying the aluminum alloy treated in step (1) for later use; (3) applying the inorganic titanium ceramic coating on the surface of the aluminum alloy obtained in step (2), and then drying it to form an aluminum alloy-inorganic titanium ceramic coating composite material for standby use; (4) subjecting the aluminum alloy-inorganic titanium ceramic coating composite material obtained in step (3) to high temperature treatment, and then applying the dispersed graphene infiltration liquid on the surface to form an aluminum alloy-inorganic titanium ceramic coating-graphene film composite material for later use; (5) attaching an inorganic titanium ceramic coating to the surface of the aluminum alloy-inorganic titanium ceramic coating-graphene film composite material obtained in step (4) and drying it, thereby completing the preparation; In step (3), the inorganic titanium ceramic coating comprises the following components calculated by mass fraction: 0.5%~2% silicon dioxide, 0.5%~2% titanium dioxide, 2%~4% aluminum oxide fiber, 0.5%~2% cerium oxide, 0.2%~0.5% inorganic vitrified microspheres, 1%~2% attapulgite, and the balance is solvent.
2. The method for preparing an aluminum alloy-inorganic titanium ceramic-graphene composite material according to claim 1, characterized in that: In step (1), the degreasing / etching agent comprises the following components calculated by mass fraction: 10%~20% potassium hydroxide, 5%~10% anhydrous sodium metasilicate, 1%~5% sodium gluconate, 1%~5% disodium ethylenediaminetetraacetate, 5%~10% fatty alcohol polyether, and the balance is water.
3. The method for preparing an aluminum alloy-inorganic titanium ceramic-graphene composite material according to claim 1, characterized in that: In step (1), the dilution is to dilute the degreasing / etching agent by 10 to 20 times, which is used to remove oil and dust on the surface and etch the surface at the same time; the immersion time is 5 to 15 minutes, and the aluminum alloy etching amount is greater than 2.0g / m 2 .
4. The method for preparing an aluminum alloy-inorganic titanium ceramic-graphene composite material according to claim 1, characterized in that: In step (3), the thickness of the inorganic titanium ceramic coating layer is 15-30 μm.
5. The method for preparing an aluminum alloy-inorganic titanium ceramic-graphene composite material according to claim 1, characterized in that: In step (4), the temperature of the high temperature treatment is 850°C.
6. The method for preparing an aluminum alloy-inorganic titanium ceramic-graphene composite material according to claim 1, characterized in that: In step (4), the graphene infiltration liquid includes graphene powder and nano bamboo charcoal powder, and the mass ratio of the graphene powder to the nano bamboo charcoal powder is 1:
3.
7. The method for preparing an aluminum alloy-inorganic titanium ceramic-graphene composite material according to claim 1, characterized in that: The graphene infiltration liquid needs to be acidified, and the process of the acidification treatment is as follows: concentrated sulfuric acid and fuming nitric acid are mixed in a mass ratio of 1:2, expandable graphite is placed in the solution and magnetically stirred to obtain a graphene oxide solution, the graphene oxide is concentrated and adjusted to a concentration of 10 mg / ml, and then the graphene oxide solution is coated on a substrate treated with surface activity, and after drying for 24 hours, a graphene oxide film is obtained, and then reduced at 80°C in an atmosphere of hydroiodic acid and pressed to obtain a graphene high thermal conductivity film; the thickness of the graphene film layer is 0.1 mm to 0.2 mm.
8. An aluminum alloy-inorganic titanium ceramic-graphene composite material prepared using the preparation method described in any one of claims 1 to 7.
9. An application of an aluminum alloy-inorganic titanium ceramic-graphene composite material prepared by the preparation method described in any one of claims 1 to 7 in the fields of medical equipment, civilian household appliances, and health and physiotherapy.