A bipolar conductive polymer and its preparation method and application
By using bipolar conductive polymers prepared under a protective atmosphere in supercapacitors, the voltage range and energy density of electrode materials are expanded, the problem of low energy density caused by the narrow voltage range in the existing technology is solved, and a more efficient High specific capacitance and electrochemical performance.
Patent Information
- Application Number
- CN202310120277.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-02-09
AI Technical Summary
Existing supercapacitors have low energy density due to the limited voltage range of conductive polymer electrode materials, making it difficult to meet high-power energy storage needs.
Bipolar conductive polymers are prepared by reacting diphenyltetracarboxylic dianhydride and aminemethyl EDOT at a specific molar ratio and temperature under a protective atmosphere, and the material is applied in supercapacitors through electrochemical polymerization to form a bipolar conductive polymer. Electrode materials with polar doping capabilities.
It has achieved good p-doping redox properties of the conductive polymer film, expanded the forward voltage range to 1.5V, and has negative n-doping capabilities, increasing the specific capacitance and solving the problem of low energy density caused by the narrow voltage range. .
Smart Images

Figure CN116153673B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of conductive polymers, and in particular to a bipolar conductive polymer and a preparation method and application thereof. Background Art
[0002] With the rapid consumption of global energy, energy storage is particularly important. Supercapacitors are a very promising high-power charge-discharge energy storage device. Supercapacitors are widely used in new energy vehicles, military industry, electronic devices and other fields due to their high power density. Supercapacitor electrode materials mainly include three types, including carbon materials, metal oxides, and conductive polymers. Conductive polymer materials mainly include polyaniline, polypyrrole, polythiophene, PEDOT and its derivatives. Conductive polymer-based electrode materials have become the most promising type of supercapacitor electrode materials due to their easy structural modification, wide voltage window, and intelligence brought by color changes during the charge and discharge process.
[0003] Conductive polymer electrode materials, as doped pseudocapacitor electrode materials, have the advantages of good conductivity, modifiable structure, and easy processing, and have attracted widespread attention. However, most of the current research is on p-type (oxidation) doped conductive polymers, such as polyaniline and polypyrrole, and the voltage range is limited to the positive direction. Therefore, how to improve the working voltage and energy density of the device is an urgent problem to be solved. Summary of the invention
[0004] The purpose of the present invention is to provide a bipolar conductive polymer and a preparation method and application thereof, so as to solve the problem of low energy density of existing supercapacitors.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a bipolar conductive polymer, comprising the following steps:
[0007] Under a protective atmosphere, biphenyltetracarboxylic dianhydride, aminomethyl EDOT and a solvent are mixed and reacted to obtain a bipolar conductive polymer;
[0008] Among them, the structure of biphenyltetracarboxylic dianhydride is as follows:
[0009]
[0010] The structure of aminomethyl EDOT is shown below:
[0011]
[0012] Preferably, in the above method for preparing a bipolar conductive polymer, the molar ratio of biphenyltetracarboxylic dianhydride to aminomethyl EDOT is 1:3 to 1:5; and the mass volume ratio of aminomethyl EDOT to solvent is 1 g:8 to 10 mL.
[0013] Preferably, in the above method for preparing a bipolar conductive polymer, the reaction temperature is 120-140° C. and the reaction time is 12-24 hours.
[0014] Preferably, in the above-mentioned method for preparing a bipolar conductive polymer, after the reaction is completed, post-treatment is further included; the post-treatment includes: cooling to room temperature, filtering, drying, eluting, purifying, and distilling under reduced pressure.
[0015] Preferably, in the above-mentioned method for preparing a bipolar conductive polymer, the stationary phase for elution and purification is 300-400 mesh silica gel, and the mobile phase is a mixture of dichloromethane and ethyl acetate in a volume ratio of 3:1.
[0016] The present invention also provides a method for preparing a bipolar conductive polymer, wherein the bipolar conductive polymer has the following structure:
[0017]
[0018] The present invention also provides an application of a bipolar conductive polymer in preparing a supercapacitor electrode material.
[0019] Preferably, in the above application, the method for preparing the supercapacitor electrode material comprises the following steps:
[0020] The bipolar conductive polymer is used as a monomer and tetrabutylammonium hexafluorophosphate is used as a supporting electrolyte. A film is prepared by electrochemical polymerization in a mixed solvent to obtain a supercapacitor electrode material.
[0021] Preferably, in the above application, the mass volume ratio of the monomer and the mixed solvent is 1g:0.33~0.5L; the concentration of the supporting electrolyte in the mixed solvent is 0.05~0.1mol / L; and the mixed solvent is a mixture of dichloromethane and acetonitrile in a volume ratio of 4:1.
[0022] Preferably, in the above application, the parameters of the electrochemical polymerization for preparing the thin film are: the scanning voltage range is -0.3 to 1.6 V, the polymerization scanning rate is 100 to 150 mV, and the number of scanning circles is 10 to 15 circles.
[0023] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0024] The bipolar conductive polymer film of the present invention has been subjected to electrochemical testing, and the results show that the film has good p-doping redox properties, a forward voltage of 1.5V, a negative n-doping capability of -2V, and good specific capacitance, and can be applied to the field of supercapacitors, solving the problem of low energy density caused by a narrow voltage range in the current field of supercapacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the description of the embodiments or the prior art are briefly introduced below.
[0026] Figure 1 is the H NMR spectrum of the bipolar conductive polymer of Example 1;
[0027] Figure 2 is a mass spectrum of the bipolar conductive polymer of Example 1;
[0028] Figure 3 The cyclic voltammetry electrochemical polymerization curve of the supercapacitor electrode material of Example 2;
[0029] Figure 4 This is a forward cyclic voltammetry curve of the supercapacitor electrode material of Example 2;
[0030] Figure 5 This is a negative cyclic voltammetry curve of the supercapacitor electrode material of Example 2;
[0031] Figure 6 This is a forward charge and discharge curve diagram of the supercapacitor electrode material of Example 2. DETAILED DESCRIPTION
[0032] The present invention provides a method for preparing a bipolar conductive polymer, comprising the following steps:
[0033] Under a protective atmosphere, biphenyltetracarboxylic dianhydride, aminomethyl EDOT and a solvent are mixed and reacted to obtain a bipolar conductive polymer;
[0034] Among them, the structure of biphenyltetracarboxylic dianhydride is as follows:
[0035]
[0036] The structure of aminomethyl EDOT is shown below:
[0037]
[0038] In the present invention, the molar ratio of the biphenyltetracarboxylic dianhydride to aminomethyl EDOT is preferably 1:3 to 1:5, more preferably 1:3.2 to 1:4.6, and more preferably 1:3.8; the mass volume ratio of aminomethyl EDOT to the solvent is preferably 1 g:8 to 10 mL, more preferably 1 g:8.4 to 9.7 mL, and more preferably 1 g:9.1 mL.
[0039] In the present invention, the solvent is preferably propionic acid.
[0040] In the present invention, the protective atmosphere is preferably nitrogen.
[0041] In the present invention, the reaction temperature is preferably 120-140°C, more preferably 124-136°C, and more preferably 127°C; the reaction time is preferably 12-24h, more preferably 15-21h, and more preferably 18h.
[0042] In the present invention, after the reaction is completed, post-treatment is also included; the post-treatment includes: cooling to room temperature, filtering, drying, eluting, purifying, and distilling under reduced pressure.
[0043] In the present invention, the stationary phase for elution purification is preferably 300-400 mesh silica gel, and the mobile phase is preferably a mixture of dichloromethane and ethyl acetate in a volume ratio of 3:1.
[0044] The present invention also provides a method for preparing a bipolar conductive polymer, wherein the bipolar conductive polymer has the following structure:
[0045]
[0046] The present invention also provides an application of a bipolar conductive polymer in preparing a supercapacitor electrode material.
[0047] In the present invention, the method for preparing the supercapacitor electrode material comprises the following steps:
[0048] The bipolar conductive polymer is used as a monomer and tetrabutylammonium hexafluorophosphate is used as a supporting electrolyte. A film is prepared by electrochemical polymerization in a mixed solvent to obtain a supercapacitor electrode material.
[0049] In the present invention, the mass volume ratio of the monomer and the mixed solvent is preferably 1 g: 0.33-0.5 L, more preferably 1 g: 0.39-0.46 L, and more preferably 1 g: 0.42 L; the concentration of the supporting electrolyte in the mixed solvent is preferably 0.05-0.1 mol / L, more preferably 0.07-0.09 mol / L, and more preferably 0.08 mol / L.
[0050] In the present invention, the mixed solvent is preferably a mixture of dichloromethane and acetonitrile in a volume ratio of 4:1.
[0051] In the present invention, the parameters for preparing the film by electrochemical polymerization are: the scanning voltage range is preferably -0.3 to 1.6 V; the polymerization scanning rate is preferably 100 to 150 mV, more preferably 105 to 145 mV, and more preferably 110 mV; the number of scanning circles is preferably 10 to 15 circles, more preferably 11 to 14 circles, and more preferably 13 circles.
[0052] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] Example 1
[0054] This embodiment provides a bipolar conductive polymer, the structure of which is shown below:
[0055]
[0056] The preparation method comprises the following steps:
[0057]
[0058] Under nitrogen protection, biphenyltetracarboxylic dianhydride (0.6 g, 2 mmol) was dissolved in propionic acid solvent (15 mL), and aminomethyl EDOT (1.7 g, 10 mmol) was added thereto. The mixture was reacted at 140°C for 24 h. After the reaction was completed, the mixture was cooled to room temperature, and the reaction product was poured into 100 mL of water. The solid phase was filtered out by vacuum filtration. After the solid phase was dried, it was purified by column chromatography using 300-400 mesh silica gel as the stationary phase and a mixed solvent of dichloromethane / ethyl acetate in a volume ratio of 3:1 as the mobile phase for elution and purification. The eluate of the target product was collected, and the mixed solvent of dichloromethane / ethyl acetate was removed by reduced pressure distillation to finally obtain 0.2 g of the target yellow solid product bipolar conductive polymer.
[0059] The results of H NMR and MS characterization of bipolar conductive polymers are shown in Figures 1-2 As shown. MS (M+1) characterization measured 601. H NMR spectrum 1 HNMR (400MHz, CDCl3) δ8.16(s,2H),8.04(s,4H),6.37(s,4H),4.54(s,2H),4.28(s,2H),4.15(s,2H),4.08(s,2H),3.97(s,2H).
[0060] Example 2
[0061] This embodiment provides a supercapacitor electrode material, and the preparation method includes the following steps:
[0062] The bipolar conductive polymer prepared in Example 1 was used as a monomer, and tetrabutylammonium hexafluorophosphate was used as a supporting electrolyte, which was dissolved in a mixed solvent of dichloromethane and acetonitrile with a volume ratio of 4:1, wherein the concentration of the supporting electrolyte in the mixed solvent was 0.1 mol / L, and the mass volume ratio of the monomer to the mixed solvent was 1 g:0.33 L; a three-electrode system was adopted, with ITO as the working electrode, platinum wire as the counter electrode, and Ag / Ag + As a reference electrode, in the cyclic voltammetry scanning voltage range of -0.3 to 1.6 V, the polymerization scan rate was set to 100 mV, and the polymerization scan was 10 cycles to obtain a bipolar conductive polymer film, which is the supercapacitor electrode material. The cyclic voltammetry electrochemical polymerization curve is shown in Figure 3 shown.
[0063] The bipolar conductive polymer film prepared above was subjected to electrochemical testing, using 0.1 mol / L lithium perchlorate as the supporting electrolyte, acetonitrile as the solvent, and a three-electrode system. The positive and negative cyclic voltammetry curves are shown in Figures 4-5 As shown. Figures 4-5 It can be seen that the forward voltage can reach 1.5V and the negative voltage can reach -2V. The bipolar conductive polymer film exhibits good capacitive behavior. Figure 6 As shown, it can be seen that at 0.05mA / cm 2 At this current density, its area specific capacitance is 0.93mF / cm 2 .
[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a bipolar conductive polymer, characterized in that: The following steps are involved: Under a protective atmosphere, biphenyltetracarboxylic dianhydride, aminomethyl EDOT and a solvent are mixed and reacted to obtain a bipolar conductive polymer; Among them, the structure of biphenyltetracarboxylic dianhydride is as follows: The structure of aminomethyl EDOT is shown below: The structure of a bipolar conducting polymer is shown below:
2. The method for preparing a bipolar conductive polymer according to claim 1, characterized in that: The molar ratio of the biphenyltetracarboxylic dianhydride to the aminomethyl EDOT is 1:3 to 1:5; the mass volume ratio of the aminomethyl EDOT to the solvent is 1 g:8 to 10 mL.
3. A method for preparing a bipolar conductive polymer according to claim 1 or 2, characterized in that: The reaction temperature is 120-140° C. and the reaction time is 12-24 hours.
4. The method for preparing a bipolar conductive polymer according to claim 3, characterized in that: The reaction also includes post-processing after completion; the post-processing includes: cooling to room temperature, filtering, drying, eluting, purifying, and distilling under reduced pressure.
5. The method for preparing a bipolar conductive polymer according to claim 4, characterized in that: The stationary phase for elution purification is 300-400 mesh silica gel, and the mobile phase is a mixture of dichloromethane and ethyl acetate in a volume ratio of 3:
1.
6. Use of a bipolar conductive polymer obtained by the method for preparing a bipolar conductive polymer according to claim 1 in preparing a supercapacitor electrode material.
7. The use according to claim 6, characterized in that: The method for preparing the supercapacitor electrode material comprises the following steps: The bipolar conductive polymer is used as a monomer and tetrabutylammonium hexafluorophosphate is used as a supporting electrolyte. A film is prepared by electrochemical polymerization in a mixed solvent to obtain a supercapacitor electrode material.
8. The use according to claim 7, characterized in that: The mass volume ratio of the monomer and the mixed solvent is 1g:0.33-0.5L; the concentration of the supporting electrolyte in the mixed solvent is 0.05-0.1mol / L; and the mixed solvent is a mixture of dichloromethane and acetonitrile in a volume ratio of 4:
1.