Polypropylene composition, preparation method thereof and articles made therefrom
The high stereoregularity polypropylene composition prepared through a specific catalyst system and polymerization process solves the problem of balancing impact resistance and high gloss of existing polypropylene materials, achieves a combination of high gloss and low haze, and simplifies production. process and reduce costs.
Patent Information
- Application Number
- CN202180056674.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-27
- Filing Date
- 2021-08-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-08-20
AI Technical Summary
It is difficult for existing polypropylene materials to achieve high gloss and low haze while maintaining impact resistance, and cannot meet the requirements of specific application fields. The production process is complex and costly.
Through specific catalyst systems and polymerization process conditions, a composition of 70-95% crystalline homopolypropylene and 5-30% ethylene-propylene elastic copolymer is prepared to form a polypropylene composition with high stereoregularity, achieving Combination of high gloss and good impact resistance.
It achieves high gloss (glossiness at 60° angle ≥80%) and low haze of polypropylene materials, while also having good mechanical properties, such as high flexural modulus and heat distortion temperature, simplifying the production process and reducing costs.
Smart Images

Figure CN116157468B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polyolefins, and in particular relates to a polypropylene composition, a method for preparing the polypropylene composition, and a product prepared from the polypropylene composition. Background Art
[0002] Polypropylene resin is widely used in the home appliance and automotive industries. Its advantages lie in that it can not only replace metals and engineering plastics, but also has the characteristics of easy recycling, light weight and relatively low price. These application fields require materials to have excellent mechanical properties (rigidity and toughness) and ideal glossiness to obtain the aesthetic effect of the products. High-gloss polypropylene is currently gradually replacing materials such as HIPS and ABS, and is used in various fields such as rice cookers, electric kettles, microwave ovens, vacuum cleaners, washing machines and other home appliance shells, automotive interior parts, children's toys, and home storage.
[0003] In addition, due to the good mechanical properties and chemical stability of polypropylene materials, the technology of using it to make medical disposable syringes has become increasingly mature. With the development of society, the demand for flushing syringes has also increased. Flushing syringes need to be pre-filled with liquid medicine and need to be resistant to high-temperature steam sterilization without deformation. Polypropylene is required to have the properties of high heat deformation temperature, high modulus, high impact resistance, high gloss and low haze.
[0004] Homopolymer and random copolymer polypropylene have high gloss, but poor impact resistance, and cannot meet the requirements of high toughness. Although the mechanical properties of homopolymer and random copolymer polypropylene can be improved by adding elastomers such as POE, the gloss will be affected, and the modification process is complicated and costly.
[0005] Impact-resistant polypropylene has a multiphase structure, so its toughness is ideal, and it can have both high modulus and high impact. However, due to the presence of the rubber phase, the haze of its products is usually high and the gloss is low, and it cannot meet the high gloss requirement of gloss>80% (60° angle gloss). In addition, due to its multiphase structure, the gloss of impact-resistant polypropylene cannot be significantly improved by adding nucleating agents, changing processing conditions, etc., and it must be adjusted and optimized based on its own structure.
[0006] CN104448538A discloses a polypropylene composition having both transparency and impact resistance. Polypropylene with good transparency usually has a high gloss. In the document, a specific ZN catalyst is selected to realize the synthesis of a polypropylene composition with a high ethylene-propylene elastomeric copolymer content (30-60% by weight) by continuous polymerization. The rubber particle size in the transparent impact-resistant polypropylene product is very small, and the crystallization of the rubber relative to the homopolymerized polypropylene matrix will have a certain impact, thereby affecting the rigidity of the polypropylene, so the modulus of the transparent impact-resistant polypropylene product is usually low.
[0007] CN109422958A discloses a high-flow, high-rigidity and high-toughness polyolefin composition and a preparation method thereof. In the polyolefin composition, the ethylene-propylene copolymer contains 40-50% by weight of high ethylene units. The impact-resistant polypropylene has good rigidity and toughness, but due to the limitation of its rubber phase structure, the glossiness of the impact-resistant polypropylene is low (less than 80%) and cannot reach the level of high gloss.
[0008] CN1321178A discloses an impact-resistant polypropylene composition having high modulus, high impact and low fog, but the rubber phase of the impact-resistant polymer is an ethylene-butene copolymer, which cannot be produced on existing domestic polypropylene devices.
[0009] Therefore, it is necessary to find a polypropylene composition that can maintain the good rigidity-toughness balance of impact-resistant polypropylene while having high gloss or low haze, so as to meet the requirements of specific application fields and expand the application range of the polypropylene composition. At the same time, the polypropylene composition should be able to be produced on existing industrial equipment. Summary of the invention SUMMARY OF THE INVENTION
[0011] In view of the prior art as described above, the object of the present invention is to provide a polypropylene composition having both high gloss and good impact resistance, in particular, having high gloss, high rigidity, high toughness and low shrinkage properties.
[0012] Another object of the present invention is to provide a method for preparing the polypropylene composition, which can be implemented on existing industrial devices, especially can directly obtain the polypropylene composition through a continuous polymerization process. The method does not require complex modification, so it is simple, low-cost and environmentally friendly.
[0013] According to the present invention, by adopting a specific catalyst system and adjusting specific polymerization process conditions, a composition of homopolypropylene with high stereoregularity and ethylene-propylene elastic copolymer with a specific composition is obtained, wherein the composition has a specific microstructure comprising a continuous matrix phase of homopolypropylene and an ethylene-propylene elastic copolymer rubber phase dispersed therein, thereby achieving the above-mentioned purpose.
[0014] Therefore, a first aspect of the present invention provides a polypropylene composition comprising:
[0015] (a) 70-95 wt% of a crystalline homopolymer polypropylene as component A, wherein the isotactic pentad fraction is 96% or more, preferably 97% or more; the crystalline homopolymer polypropylene forms a continuous matrix phase in the polypropylene composition;
[0016] (b) 5-30 wt% of an ethylene-propylene elastic copolymer as component B, the ethylene-propylene elastic copolymer containing 20-35 wt%, preferably 25-35 wt%, of ethylene structural units, and 65-80 wt%, preferably 65-75 wt%, of propylene structural units, based on the total weight of the ethylene-propylene elastic copolymer; the ethylene-propylene elastic copolymer forms a dispersed rubber phase in the continuous matrix phase;
[0017] The ratio of the melt mass flow rate of the crystalline homopolypropylene to that of the polypropylene composition measured at 230° C. and a load of 2.16 kg according to GB / T3682.1-2018 is 0.5-2.0, preferably 0.9-1.5.
[0018] The second aspect of the present invention provides a method for preparing the polypropylene composition according to the first aspect of the present invention, comprising the following steps:
[0019] (1) contacting a propylene monomer with a stereoselective Ziegler-Natta catalyst under a first olefin polymerization condition, and removing unreacted monomers from a mixture obtained after the contact reaction to obtain a product a, wherein the product a comprises component A;
[0020] (2) Under the second olefin polymerization conditions, in the gas phase, ethylene monomer and propylene monomer are contacted with the product a obtained in step (1) for reaction, and unreacted monomers are removed from the mixture obtained after the contact reaction to obtain a product b containing component A and component B as the polypropylene composition.
[0021] The third aspect of the present invention provides a product, which is prepared from the polypropylene composition of the first aspect.
[0022] Other aspects and advantageous effects of the present invention will be apparent from the following detailed description of the invention and specific embodiments thereof in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The SEM photograph of the injection-molded sample of Example A1 at a position within a 10% thickness range from the surface of the product is shown.
[0024] Figure 2 The SEM photograph of the injection-molded sample of Example A1 shows the position of the core portion outside the 10% thickness range from the surface of the product.
[0025] Figure 3 The SEM photograph of the MFR strip of Example A1 is shown (which can be considered to be close to the SEM photograph of the pellets).
[0026] Figure 4The SEM photograph of the core portion of the injection-molded sample of Example B1, which is located outside the 10% thickness range from the surface of the product, is shown.
[0027] Figure 5 A SEM photograph of the pellets of Example B1 is shown.
[0028] Figure 6 The SEM photograph of the core portion of the injection molded sample of Comparative Example A2, which is outside the 10% thickness range from the surface of the product, is shown.
[0029] Figure 7 A SEM photograph of the pellets of Comparative Example A2 is shown. DETAILED DESCRIPTION OF THE INVENTION
[0031] In a first aspect, the present invention provides a polypropylene composition comprising:
[0032] (a) 70-95 wt% of a crystalline homopolymer polypropylene as component A, wherein the isotactic pentad fraction is 96% or more, preferably 97% or more; the crystalline homopolymer polypropylene forms a continuous matrix phase in the polypropylene composition;
[0033] (b) 5-30 wt% of an ethylene-propylene elastic copolymer as component B, the ethylene-propylene elastic copolymer containing 20-35 wt%, preferably 25-35 wt%, of ethylene structural units and 65-80 wt%, preferably 65-75 wt%, of propylene structural units, based on the total weight of the ethylene-propylene elastic copolymer; the ethylene-propylene elastic copolymer forms a dispersed rubber phase in the continuous matrix phase;
[0034] The ratio of the melt mass flow rate of the crystalline homopolypropylene to that of the polypropylene composition measured at 230° C. and a load of 2.16 kg according to GB / T3682.1-2018 is 0.5-2.0, preferably 0.9-1.5.
[0035] Component A in the polypropylene composition of the present invention is a crystalline homopolypropylene, and its isotactic pentad fraction is 96% or more, preferably 97% or more, for example 97.1%, 97.2%, 97.3%, 97.4%, 97.5%, 97.6%, 97.7%, 97.8%, 97.9%, 98.0%, 98.5%, 99.0% and the ranges formed by these numerical points. The crystalline homopolypropylene is a high crystalline homopolypropylene.
[0036] The isotactic pentad number is given by 13 C NMR measurement, the solvent used was deuterated o-dichlorobenzene.
[0037] The crystalline homopolypropylene forms a continuous phase in the polypropylene composition, which is a matrix phase, also called "base phase". The matrix phase is substantially formed by component A.
[0038] Component B in the polypropylene composition of the present invention is an ethylene-propylene elastic copolymer.
[0039] The ethylene-propylene elastic copolymer contains 20-35 wt%, preferably 25-35 wt% of ethylene structural units and 65-80 wt%, preferably 65-75 wt% of propylene structural units, based on the total weight of the ethylene-propylene elastic copolymer.
[0040] The ethylene-propylene elastomeric copolymer is dispersed in the continuous matrix phase and forms a rubber phase, which is a dispersed phase. The rubber phase is substantially formed by component B.
[0041] The morphology of the rubber phase formed by the ethylene-propylene elastic copolymer in the polypropylene composition of the present invention is similar to the morphology of the rubber phase obtained by conventional methods. When no orientation force is applied, the rubber phase in the polypropylene composition of the present invention is a spherical or nearly spherical particle. The spherical and nearly spherical means that the aspect ratio of the rubber phase particles is basically in the range of 1-2. "Basically" means that at least 90% of the rubber phase particles have an aspect ratio in the range of 1-2. The aspect ratio is the ratio of the longest dimension of the particle (the distance between the two farthest points on the particle outline, i.e., the longitudinal axis) and the length of the straight line with the longest distance between the intersection points of the straight line perpendicular to the longitudinal axis that intersects the particle outline (horizontal axis). Preferably, when no orientation force is applied, at least 95% of the rubber phase particles have an aspect ratio of 1-2.
[0042] The size of the rubber phase obtained by the present invention is smaller than that of the rubber phase obtained by conventional methods. When no orientation force is applied, the average size of the rubber phase particles in the polypropylene composition of the present invention can be 0.03-3.0 μm, preferably 0.05-2.0 μm, more preferably 0.05-1.5 μm, more preferably 0.1-1.5 μm.
[0043] The average size of the rubber phase particles is measured by a scanning electron microscope (SEM) method. Specifically, for spherical rubber phase particles, the diameter of the rubber phase particles in the SEM photo is measured; for nearly spherical rubber phase particles or rubber phase particles after being acted upon by an orientation force, the longest dimension of the particle (the distance between the two points on the particle contour that are the farthest apart) is measured, and the average value of the above dimensions of 50 rubber phase particles is obtained by observing the SEM photo as the average size of the rubber phase or the average size of the rubber phase particles. When measuring the average size of the rubber phase particles after being acted upon by an orientation force, the observation surface of the SEM is parallel to the direction of the orientation force (external field force), such as the injection molding direction.
[0044] In addition, unlike conventional rubber phases, the rubber phase in the polypropylene composition of the present invention can at least partially (or even completely) deform and form an oriented structure under the action of the orientation force. After the orientation force is removed and the sample is formed, the rubber phase can still maintain the oriented structure.
[0045] The orientation force refers to an external field force that can cause an object to be oriented, and the orientation refers to the parallel arrangement of the object along the direction of the external field force. The external field force can be a tensile stress and / or a shear stress, such as a force applied to the polypropylene composition by the process itself for preparing the product, such as a force applied to the polypropylene composition during a process such as injection molding.
[0046] The term "oriented structure" herein refers to the longitudinal axes of rubber phase particles that are deformed and elongated under the action of the orientation force and arranged parallel to each other along a certain direction. A small amount of rubber phase particles located in a local area of the composition and arranged in a different direction that is inconsistent with the overall arrangement direction of the rubber phase particles in the entire composition due to the preparation process is excluded here.
[0047] As used herein, "parallel arrangement" includes substantially parallel conditions wherein the longitudinal axes of the rubber phase particles are at an angle of less than about 10 degrees, preferably less than about 5 degrees, relative to each other.
[0048] Preferably, after the orientation force acts, at least 80% of the rubber phase particles form an oriented structure based on the total number of rubber phase particles in the SEM image, excluding rubber phase particles that cannot be clearly observed due to the preparation process or SEM method.
[0049] After the orientation force has been applied, at least 50% of the rubber phase particles in the polypropylene composition of the present invention may achieve an aspect ratio greater than 2, based on the total number of rubber phase particles in the SEM picture.
[0050] The rubber phase in the polypropylene composition of the present invention can be deformed and oriented not only in the surface layer of the composition (e.g., within the range of 10% thickness of the injection molded sample from the surface of the product, i.e., the region with a distance from the surface of the product of less than or equal to 10% of the thickness) after the action of the orientation force, but also in the interior of the composition. However, the rubber phase in the interior of the composition, especially in the core part (the region with a distance from the surface of the product of more than 10% of the thickness) outside the range of 10% thickness of the injection molded sample from the surface of the product, is less likely to be deformed and oriented. When the ratio of the melt mass flow rate of the crystalline homopolypropylene to the polypropylene composition is close to 1, the deformation and orientation of the rubber phase in the core part can be advantageously easily achieved.
[0051] In the polypropylene composition of the present invention, the ratio of the melt mass flow rate of the crystalline homopolypropylene to that of the polypropylene composition measured at 230° C. and a load of 2.16 kg according to GB / T3682.1-2018 may be 0.5-2.0, preferably 0.9-1.5.
[0052] The crystalline homopolypropylene forming the matrix phase may have a melt mass flow rate of 5-200 g / 10 min, preferably 10-100 g / 10 min, at 230° C. and a load of 2.16 kg according to GB / T 3682.1-2018.
[0053] The polypropylene composition may have a melt mass flow rate of 5-100 g / 10 min, preferably 6-30 g / 10 min, and more preferably 8.89-30 g / 10 min at 230° C. and a load of 2.16 kg according to GB / T 3682.1-2018.
[0054] The intrinsic viscosity of the polypropylene composition according to the present invention may be 1.0-2.5 dL / g, preferably 1.4-2.4 dL / g, more preferably 1.52-2.08 dL / g. The intrinsic viscosity of the xylene solubles in the polypropylene composition may be 1.0-4.0 dL / g, preferably 1.11-3.65 dL / g. The ratio of the intrinsic viscosity of the xylene solubles in the polypropylene composition to the intrinsic viscosity of the crystalline homopolypropylene is preferably 0.7-2.6. The intrinsic viscosity is measured by a capillary detector.
[0055] The molecular weight distribution Mw / Mn of the polypropylene composition is preferably ≤ 5, more preferably Mw / Mn ≤ 4.5. The molecular weight distribution is determined by gel permeation chromatography (GPC) analysis relative to polystyrene standards.
[0056] According to one embodiment, the polypropylene composition according to the present invention may further comprise: (c) a nucleating agent as component C, thereby advantageously further improving the mechanical properties. The nucleating agent may be selected from at least one of carboxylic acids and metal salts thereof, sorbitols, aryl phosphates, dehydroabietic acid and salts thereof, aromatic amides, aromatic amines, rare earth compounds, condensed ring compounds with quasi-planar structures, and polymer nucleating agents. The nucleating agent is preferably a carboxylate nucleating agent and / or an aryl phosphate nucleating agent, such as Millad HPN-20E nucleating agent, Millad HPN-715 nucleating agent, Millad 600EI nucleating agent (available from Milliken & Company, USA).
[0057] Based on the total weight of the polypropylene composition, the content of the nucleating agent may be 0.05-0.3 wt %.Based on the total weight of component A and component B, the content of the nucleating agent as component C may be 0.05-3 wt %.
[0058] The polypropylene composition according to the present invention may also include other auxiliary agents conventionally used in the field of polymers, thereby giving the polypropylene composition of the present invention further advantageous properties. The other auxiliary agents may be selected from at least one of antioxidants, antistatic agents and colorants. Based on the gross weight of the polypropylene composition, the content of the other auxiliary agents may be 0.05-0.6 wt %, preferably 0.1-0.3 wt %.
[0059] The polypropylene composition according to the present invention has significantly higher gloss, and its 60° angle gloss can reach ≥80%, preferably ≥85%, and more preferably ≥90%. In a preferred embodiment, the polypropylene composition can also have a haze of ≤50%, more preferably ≤40%, thereby having both high gloss and high transparency.
[0060] The polypropylene composition according to the present invention additionally has good mechanical properties, in particular one or more, preferably all of the following properties:
[0061] 1) Parallel shrinkage ratio ≤1.15, preferably ≤1.1;
[0062] 2) Vertical shrinkage ratio ≤1.36, preferably ≤1.15;
[0063] 3) flexural modulus ≥ 1000 MPa, preferably ≥ 1300 MPa, more preferably ≥ 1400 MPa, and even more preferably ≥ 1450 MPa;
[0064] 4) Room temperature simply supported beam notched impact strength ≥5kJ / m 2 , preferably ≥6kJ / m 2 ;
[0065] 5) Heat deformation temperature ≥ 90°C, preferably ≥ 92°C.
[0066] In this article, the 60° angle gloss is measured according to GB / T 8807-1988 on injection molded samples, and the sample thickness is 2 mm. The haze is measured according to GB / T 2410-2008 on injection molded samples, and the sample thickness is 1 mm. The shrinkage is measured according to GB / T 17037.4-2003 on injection molded samples. The flexural modulus is measured according to GB / T9341-2008 on injection molded samples. The room temperature simple supported beam notched impact strength is measured according to GB / T 1043.1-2008 at 23°C on injection molded samples. The heat deformation temperature is measured according to GB / T1634.2-2004 on injection molded samples.
[0067] The polypropylene composition may be in the form of powder or pellets. The pellets may be obtained, for example, by mixing and granulating. The mixing and granulating method may be any conventional method in the art, and the present invention has no particular limitation thereto, for example, a twin-screw extruder may be used for granulation. In the pellets of the polypropylene composition of the present invention, the rubber phase remains spherical or nearly spherical.
[0068] In a second aspect, the present invention provides a method for preparing a polypropylene composition according to the present invention, comprising the following steps:
[0069] (1) contacting a propylene monomer with a stereoselective Ziegler-Natta catalyst under a first olefin polymerization condition, and removing unreacted monomers from a mixture obtained after the contact reaction to obtain a product a, wherein the product a comprises component A;
[0070] (2) Under the second olefin polymerization conditions, in the gas phase, ethylene monomer and propylene monomer are contacted with the product a obtained in step (1) for reaction, and unreacted monomers are removed from the mixture obtained after the contact reaction to obtain a product b containing component A and component B as the polypropylene composition.
[0071] In the method of the present invention, a stereoselective Ziegler-Natta catalyst can be used to prepare the highly crystalline homopolymer polypropylene with high stereoregularity, and the homopolymer together with the active catalyst is further contacted with ethylene and propylene to form a polypropylene composition of a rubber phase dispersed in a continuous matrix phase of the homopolymer.
[0072] The stereoselective Ziegler-Natta catalyst may contain:
[0073] (i) a solid catalyst component, the solid catalyst component comprising a product obtained by reacting a magnesium source, a titanium source and an internal electron donor;
[0074] (ii) an organoaluminum compound; and
[0075] (iii) Optional external electron donor.
[0076] The Ziegler-Natta catalyst preferably has a high stereoselectivity.
[0077] The solid catalyst component is used as a main catalyst in the method of the present invention. The amount of each component in the solid catalyst component can be determined as needed. Preferably, the molar ratio of the magnesium source calculated as magnesium element, the titanium source calculated as titanium element and the internal electron donor can be 1: (20-150): (0.1-0.9), preferably 1: (30-120): (0.15-0.6).
[0078] The solid catalyst component used in the method of the present invention can be commercially available, or prepared by methods known in the art, such as the method disclosed in CN106608934B.
[0079] The titanium source may be a titanium compound, for example, a compound selected from the general formula Ti(OR) 4-m X m One or more of the titanium compounds shown, wherein m is an integer of 0-4, preferably an integer of 1-4, and R can be C1-C 20 Alkyl, preferably C1-C 10 X may be halogen, preferably chlorine.
[0080] The magnesium source can be various magnesium-containing compounds that can be used as catalysts for olefin polymerization, such as magnesium halides, magnesium alcoholates or halogenated alcoholates, and magnesium halide adduct supports, etc., preferably spherical magnesium halide adduct supports, such as those prepared according to the method disclosed in Example 1 of CN1330086A or the method disclosed in CN106608934B.
[0081] The internal electron donor may be preferably selected from esters of monocarboxylic acids, esters of dicarboxylic acids, phosphate compounds, diether compounds, and combinations thereof.
[0082] In a preferred embodiment, the internal electron donor can be an ester of a monocarboxylic acid and / or an ester of a dicarboxylic acid, preferably selected from at least one of benzoate, malonic acid ester, phthalate and succinate, wherein more preferably phthalate. Phthalate includes alkyl phthalate (e.g. diisobutyl phthalate and / or dioctyl phthalate) and / or aryl phthalate (e.g. diphenyl phthalate and / or benzyl butyl phthalate). More suitable is alkyl phthalate, further preferably diisobutyl phthalate and / or dioctyl phthalate.
[0083] In this embodiment of the method of the present invention using esters of monocarboxylic acids and / or esters of dicarboxylic acids as internal electron donors, a nucleating agent is preferably used. The glossiness at 60° angle of the prepared polypropylene composition can reach ≥80%, preferably ≥85%; the parallel shrinkage can be ≤1.15, the vertical shrinkage can be ≤1.15; the flexural modulus can be ≥1000MPa, preferably ≥1300MPa, and the room temperature simple supported beam notched impact strength can be ≥5kJ / m 2 .
[0084] In another preferred embodiment of the method of the present invention, the internal electron donor may be an internal electron donor composed of a phosphate compound and a diether compound.
[0085] The molar ratio of the diether compound to the phosphate compound may be 1:(0.02-0.25), preferably 1:(0.04-0.15).
[0086] The phosphate compound can be selected from at least one of the phosphate compounds shown in formula (1),
[0087]
[0088] wherein R1, R2 and R3 are each independently selected from a C1-C4 straight chain or branched chain alkyl, a C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkyl or C7-C 20 of aralkyl.
[0089] Preferably, the phosphate compound may include, but is not limited to: at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate, triphenyl phosphate, tricresyl phosphate, triisopropylphenyl phosphate, trimethoxyphenyl phosphate, phenyl dimethyl phosphate, cresyl dibutyl phosphate, isopropylphenyl dimethyl phosphate, isopropylphenyl diethyl phosphate, isopropylphenyl dibutyl phosphate, phenyl ditolyl phosphate, phenyl diisopropylphenyl phosphate, p-cresyl dibutyl phosphate, m-cresyl dibutyl phosphate, p-cumyl dimethyl phosphate, p-cumyl diethyl phosphate, p-tert-butylphenyl dimethyl phosphate and o-cresyl p-di-tert-butylphenyl phosphate.
[0090] The diether compound can be selected from at least one of the diether compounds shown in formula (2), R 1 R 2 C(CH2OR 3 )(CH2OR 4 ) Formula (2)
[0091] Among them, R 1 and R 2 Each independently selected from hydrogen, C1-C 20 Straight or branched alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Arylalkyl or C7-C 20 Alkyl, R 3 and R 4 Each independently selected from C1-C 10 of alkyl.
[0092] Preferably, the diether compound may include, but is not limited to: 2-(2-ethylhexyl)-1,3-dimethoxypropane, 2-isopropyl-1,3-dimethoxypropane, 2-butyl-1,3-dimethoxypropane, 2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-1,3-dimethoxypropane, 2-phenyl-1,3-dimethoxypropane, 2-(2-phenylethyl)-1,3-dimethoxypropane, 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-(p-chlorophenyl)-1,3-dimethoxypropane, 2-(diphenylmethyl)-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane. 2-Methyl-2-phenyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-benzyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl ... ,2-bis(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-diphenyl-1,3-dimethoxypropane, 2,2-dibenzyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2-isobutyl-2-isopropyl-1,3-dimethoxypropane, 2-(1-methylbutyl)-2-isopropyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane , 2-phenyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2-sec-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclohexyl-2-sec-butyl-1,3-dimethoxypropane, 2-isopropyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane and at least one of 9,9-dimethoxymethylfluorene.
[0093] In this embodiment of the method of the present invention using a phosphate compound and a diether compound as the internal electron donor, a nucleating agent is preferably used. The glossiness of the prepared polypropylene composition at 60° can reach ≥85%, preferably ≥90%; and the haze is ≤50%, preferably ≤40%. In this embodiment, the parallel shrinkage of the prepared polypropylene composition can be ≤1.15, preferably ≤1.1; the flexural modulus can be ≥1400MPa, preferably ≥1450MPa; the room temperature simply supported beam notched impact strength can be ≥5kJ / m 2 , preferably ≥6kJ / m 2 ; The heat deformation temperature can be ≥90°C, preferably the heat deformation temperature is ≥92°C; the molecular weight distribution Mw / Mn is narrow, which can be ≤5, preferably the molecular weight distribution Mw / Mn≤4.5.
[0094] The present invention unexpectedly found that the polypropylene composition prepared by the catalyst system of the internal electron donor of the composite of the phosphate compound and the diether compound has higher gloss and lower haze and has comparable mechanical properties, and can have good transparency, high gloss, high rigidity, high toughness and low shrinkage properties, thereby having both good mechanical properties and aesthetic characteristics.
[0095] In the method of the present invention, an organoaluminum compound is used as a co-catalyst. It is preferably an alkylaluminum compound, including but not limited to: one or more of triethylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-hexylaluminum, diethylaluminum monochloride, di-n-butylaluminum monochloride, diisobutylaluminum monochloride, di-n-hexylaluminum monochloride, monoethylaluminum dichloride, mono-n-butylaluminum dichloride, monoisobutylaluminum dichloride and mono-n-hexylaluminum dichloride. The alkylaluminum compound is preferably a trialkylaluminum, such as at least one of triethylaluminum, tri-n-butylaluminum and triisobutylaluminum.
[0096] The catalyst system used in the method of the present invention may also include an external electron donor. The external electron donor may be an organosilicon compound, preferably having the general formula R n Si(OR') 4-n An organosilicon compound, wherein 0<n≤3, R is selected from hydrogen atom, halogen, alkyl, cycloalkyl, aryl and halogenated alkyl, and R' is selected from alkyl, cycloalkyl, aryl and halogenated alkyl.
[0097] The external electron donor may preferably include, but is not limited to, at least one of tetramethoxysilane, tetraethoxysilane, trimethylmethoxysilane, trimethylethoxysilane, trimethylphenoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methyl tert-butyldimethoxysilane, methylisopropyldimethoxysilane, diphenoxydimethoxysilane, diphenyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, cyclohexylmethyldimethoxysilane, dicyclopentyldimethoxysilane, diisopropyldimethoxysilane, diisobutyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane.
[0098] The organosilicon compound as an external electron donor can be added all at once in a system of two or more reactors operating in series, or can be added in portions at different locations; it can be added directly to the reactor, or added to equipment or pipelines related to reactor feed.
[0099] In the method of the present invention, the amounts of the solid catalyst component, the organoaluminum compound and the external electron donor can also be determined as needed. The amount ratio of the solid catalyst component to the organoaluminum compound in terms of titanium / aluminum molar ratio can be 1:(25-100). The weight ratio of the organoaluminum compound to the external electron donor can be (0-150):1, preferably (2-150):1, and more preferably (3-10):1.
[0100] In the preparation process of the catalyst used in the present invention, the organoaluminum compound and the optional external electron donor can be mixed with the solid catalyst component separately and then reacted, or the organoaluminum compound and the optional external electron donor can be premixed and then mixed with the solid catalyst component and reacted.
[0101] The catalyst used in the present invention can be directly added to the reactor, or can be added to the reactor after being pre-complexed and / or pre-polymerized as known in the art.
[0102] The pre-complexation and pre-polymerization process can be carried out in an environment with or without polymerizable monomers, such as in a separate pre-complexation or pre-polymerization reactor. When the pre-complexation reaction is carried out alone, the reactor can be in the form of a continuous stirred tank reactor, or other forms that can achieve a sufficient mixing effect, such as a loop reactor, a section of pipeline containing a static mixer, or even a section of pipeline where the material is in a turbulent state. The pre-complexation temperature can be controlled between -10°C and 60°C, preferably 0-30°C. The pre-complexation time can be controlled between 0.1-180min, preferably 5-30min.
[0103] The catalyst with or without pre-complexation can also be optionally subjected to prepolymerization treatment. The prepolymerization can be carried out continuously under liquid phase bulk conditions, or intermittently in an inert solvent. The prepolymerization reactor can be a continuous stirred tank, a loop reactor, etc. The temperature of the prepolymerization can be controlled between -10°C and 60°C, preferably 0-40°C. The multiple of the prepolymerization can be controlled between 0.5-1000 times, preferably 1.0-500 times.
[0104] In step (1) of the method of the present invention, the first olefin polymerization conditions may be liquid phase polymerization conditions or gas phase polymerization conditions, that is, the polymerization may be liquid phase polymerization or gas phase polymerization.
[0105] The liquid phase polymerization conditions may include: using hydrogen as a molecular weight regulator, a polymerization temperature of 0-150° C., preferably 40-100° C.; and a polymerization pressure higher than the saturated vapor pressure of propylene at the corresponding polymerization temperature.
[0106] The gas phase polymerization conditions may include: using hydrogen as a molecular weight regulator, a polymerization temperature of 0-150° C., preferably 40-100° C.; and a polymerization pressure greater than or equal to normal pressure, preferably 0.5-2.5 MPa.
[0107] The hydrogen / propylene ratio used in step (1) is preferably 0.0010-0.0060 mol / mol, that is, the hydrogen concentration is preferably 0.10-0.60 mol%.
[0108] In the gas phase polymerization reaction system of step (2) of the method of the present invention, the molar ratio of ethylene / (ethylene+propylene) can be 0.1-0.4 mol / mol, preferably 0.1-0.3 mol / mol, more preferably 0.1-0.25 mol / mol, and even more preferably 0.15-0.25 mol / mol. The temperature of the gas phase polymerization of olefins can be 40-100° C., preferably 60-80° C. The pressure can be 0.6-1.4 MPa, preferably 1.0-1.3 MPa. In a preferred embodiment of step (2), the hydrogen / ethylene ratio is 0.02-0.70 mol / mol, preferably 0.04-0.54 mol / mol.
[0109] In this article, pressure refers to gauge pressure.
[0110] The polymerization in steps (1) and (2) of the present invention can be carried out continuously or batchwise.
[0111] Continuous polymerization can use more than two reactors in series. The first or first few reactors prepare product a, which contains component A, especially mainly composed of component A. The reactor for preparing product a can be a liquid phase reactor or a gas phase reactor. The liquid phase reactor can be a loop reactor or a stirred tank reactor. The gas phase reactor can be a horizontal stirred bed reactor or a vertical stirred bed reactor or a fluidized bed reactor or a multi-zone circulation reactor, etc. The reactor after preparing product a is used to prepare product b or component B, and the product b contains component A and component B, especially mainly composed of components A and B. The reactor for preparing product b or component B is a gas phase reactor, which can be a horizontal stirred bed reactor or a vertical stirred bed reactor or a fluidized bed reactor, etc. The above gas phase reactors can also be arbitrarily matched and combined.
[0112] The polymerization of the present invention can also be carried out intermittently. The product a and the product b are prepared in sequence in the reactor. For the preparation of product a, polymerization can be carried out in the liquid phase or in the gas phase. For the preparation of product b or component B, polymerization needs to be carried out in the gas phase.
[0113] When the polypropylene composition of the present invention comprises a nucleating agent and other optional auxiliary agents, the nucleating agent and other auxiliary agents may be added before or during step (1), before, during or after step (2) without affecting the polymerization reaction. Preferably, the method of the present invention may further comprise step (3): mixing the product b obtained in step (2) with the nucleating agent and other optional auxiliary agents, especially mixing and granulating. The mixing and granulating method may be various conventional methods in the art, for example, granulation may be performed using a twin-screw extruder.
[0114] In particular, in the case of a catalyst system of an internal electron donor composed of a phosphate compound and a diether compound, the product b obtained in step (2) is mixed with a nucleating agent and granulated in step (3). The polypropylene composition prepared in this way can have both high gloss (60° angle gloss ≥ 85%, preferably ≥ 90%) and low haze (haze ≤ 50%, preferably ≤ 40%), thereby advantageously having both high gloss and high transparency.
[0115] The polypropylene composition prepared according to the process of the present invention can achieve a combination of good mechanical properties (high stiffness, high toughness and low shrinkage) and aesthetic properties (high gloss, even high transparency and low haze).
[0116] Compared with a catalyst system using carboxylic acid ester as an internal electron donor, a polypropylene composition prepared by a catalyst system using a phosphate compound and a diether compound as an internal electron donor has higher gloss and lower haze and has comparable mechanical properties, and can have good transparency, high gloss, high rigidity, high toughness and low shrinkage properties.
[0117] The polypropylene composition prepared according to the method of the present invention can provide raw materials with better comprehensive properties for downstream processing due to the above-mentioned favorable comprehensive properties, and has a wider application field. The preparation method of the polypropylene composition of the present invention can be implemented on existing industrial devices, especially by continuous polymerization process. The preparation method is economical and convenient.
[0118] In a third aspect, the present invention provides an article prepared from the polypropylene composition according to the present invention. In the article, the rubber phase is at least partially deformed and forms an oriented structure. In a preferred embodiment, the rubber phase is deformed, elongated and forms an oriented structure at the position of the core part within 10% thickness range from the article surface and outside 10% thickness range from the article surface, and preferably the rubber phase in the article is completely deformed and forms an oriented structure.
[0119] The article is preferably an injection molded article.
[0120] According to the present invention, after the orientation force is applied during the process of manufacturing the article (eg, injection molding), the rubber phase will be at least partially, preferably at least 80%, or even completely deformed, elongated, and form an oriented structure.
[0121] In a preferred embodiment, more than 50% of the rubber phase particles within 10% thickness range from the surface of the article have an aspect ratio greater than or equal to 4; more than 50% of the rubber phase particles in the core portion outside the 10% thickness range from the surface of the article have an aspect ratio greater than or equal to 2, based on the total number of rubber phase particles in the SEM photograph at the corresponding position.
[0122] Thus, the article of the present invention comprises an oriented structure of an ethylene-propylene elastomeric copolymer rubber phase dispersed in a highly crystalline homopolypropylene continuous phase, thereby unexpectedly improving the gloss of the article while maintaining good mechanical properties.
[0123] The product of the present invention can be used in various fields such as home appliances, household products, packaging, toys, automobile modification, medicine, etc. For example, the product of the present invention can be a product or a part of the product used in the fields of electrical appliances, household products, packaging, toys, automobiles or medicine, especially a housing of a home appliance, a household storage product, a toy, an automobile interior component or a disposable medical syringe, such as a flushing syringe. DETAILED DESCRIPTION
[0124] The present invention is further illustrated below in conjunction with embodiments, but the scope of the present invention is not limited to these embodiments.
[0125] Parameter measurement method :
[0126] Melt mass flow rate (MFR): measured according to GB / T 3682.1-2018 at 230°C and 2.16 kg load.
[0127] The molar ratio of gas in the reactor was measured by gas chromatography, ABB, Switzerland, Vista II online chromatograph.
[0128] Xylene soluble matter content: determined according to GB / T 24282-2009.
[0129] Tensile strength: measured on injection molded specimens according to GB / T 1040.1-2006.
[0130] Flexural modulus: measured on injection molded specimens according to GB / T 9341-2008.
[0131] Charpy notched impact strength: According to GB / T 1043.1-2008, the injection molded samples were measured at 23℃ and -20℃.
[0132] Rockwell hardness: Measure injection molded samples according to GB / T 3398.2-2008.
[0133] Heat deformation temperature: measured on injection molded samples according to GB / T 1634.2-2004.
[0134] Gloss: Measure injection molded samples according to GB / T 8807-1988, sample thickness 2mm.
[0135] Shrinkage: Measure the injection molded samples according to GB / T 17037.4-2003.
[0136] Haze: Measure injection molded samples according to GB / T 2410-2008, with a sample thickness of 1 mm.
[0137] Molecular weight distribution (GPC analysis): measured by PL-GPC 220 high temperature gel permeation chromatograph produced by Agilent Technologies, USA. Temperature 150°C, 3 PLgel 13μm Olexis columns, 300.0mm×7.5mm, mobile phase 1,2,4-trichlorobenzene (with 0.25g / L antioxidant 2,6-dibutyl-p-cresol added), flow rate 1.0mL / min, IR5 infrared detector, sample concentration of about 1mg / mL, and universal calibration using narrow distribution polystyrene standards.
[0138] Isotactic pentad fraction: Use Bruker AVANCEⅢ400MHz NMR spectrometer, 10mm probe, deuterated o-dichlorobenzene as solvent. About 200mg sample / 2.5ml solvent, the sample tube is heated in a 130-140℃ oil bath until the sample is dissolved to form a uniform solution. Test conditions are: probe temperature 125℃, 90° pulse, sampling time AQ 5 seconds, delay time D1 10 seconds.
[0139] Ethylene structural unit content and propylene structural unit content: measured by infrared method, using Magna-IR 200 infrared spectrometer produced by Nicolet Company of the United States.
[0140] SEM photos: Sample pellets or injection molded samples, injection molding conditions in accordance with GB / T17037.1-2019, after liquid nitrogen cooling, brittle fracture or ultra-thin sectioning, the section is immersed in xylene solution, the rubber phase is etched away, and then the surface is cleaned and dried before SEM testing. The surface is sprayed with gold before testing. A Japanese HITACHI S-4800 cold field emission scanning electron microscope is used.
[0141] Average size of rubber phase particles: measured by SEM method. For spherical rubber phase particles, the diameter of the rubber phase particles in the SEM photo is measured; for nearly spherical rubber phase particles or rubber phase particles after the action of orientation force, the longest dimension of the particle is measured (the distance between the two points on the particle contour that are farthest apart), and the average value of the above dimensions of 50 rubber phase particles is obtained by SEM photo observation as the average size of the rubber phase particles. When measuring the average size of rubber phase particles after the action of orientation force, the observation surface of SEM is parallel to the injection direction.
[0142] Intrinsic viscosity: measured using a capillary detector (capillary detector in CRYSTEX instrument produced by PolymerChar, Spain).
[0143] Example A1
[0144] (1) Preparation of polypropylene composition
[0145] The polymerization reaction was carried out on a polypropylene pilot plant. The polymerization method and steps are as follows:
[0146] Preparation of main catalyst Cat-1: According to the method of Example 1 in CN106608934B, 150mL white oil (purchased from Guangzhou Mingen Petrochemical Co., Ltd., by weight, with a water content of less than 50ppm), 300mL methyl silicone oil (purchased from Dow Corning, with a viscosity of 300 centipoise / 20°C, by weight, with a water content of less than 50ppm), 30g magnesium chloride containing 0.44wt% water (purchased from Fushun Xinyi Titanium Factory), 50mL anhydrous ethanol (purchased from Beijing Chemical Plant, by weight, with a water content of less than 100ppm) and 1mL 2-methoxybenzoyl chloride (purchased from TOKYOKASEI KOGYO CO.LTD) were added to a 1000mL reactor, and the temperature was raised to 125°C under stirring. After 3 hours of isothermal reaction, the mixture was pressed into 2L hexane (by weight, water content less than 5ppm) pre-cooled to -30°C under a pressure of 0.3MPa through a discharge pipeline pre-installed with 4 layers of metal mesh with an aperture of 75μm (each layer with a thickness of 0.1mm) for rapid cooling. The liquid was filtered off, and the obtained solid was washed 5 times with 300mL of hexane and vacuum dried at 30°C for 1.5 hours to obtain a spherical magnesium halide adduct. In a 300mL glass reaction bottle, 10mL of hexane and 90mL of titanium tetrachloride were added in sequence under nitrogen protection, cooled to -20°C, 8.0g of spherical magnesium halide adduct was added, and stirred at -20°C for 30 minutes. Then, the temperature was slowly raised to 110°C, and 1.5mL of diisobutyl phthalate was added during the heating process. After 30 minutes of isothermal reaction at 110°C, the liquid was filtered off. Add 80 mL of titanium tetrachloride, heat to 120°C, maintain at 120°C for 30 minutes, and filter out the liquid; then, add another 80 mL of titanium tetrachloride, heat to 120°C, maintain at 120°C for 30 minutes, and filter out the liquid. Finally, wash the obtained solid with 60°C hexane for 5 times (80 mL of hexane per time), and vacuum dry the obtained solid.
[0147] Prepolymerization: The main catalyst Cat-1, the internal electron donor is diisobutyl phthalate, the cocatalyst (triethylaluminum), and the external electron donor diisopropyldimethoxysilane (DIPMS) are pre-contacted at 10°C for 20 minutes, and then continuously added to the prepolymerization reactor for prepolymerization reaction. The flow rate of triethylaluminum (TEAL) is 6g / hr, the flow rate of diisopropyldimethoxysilane is 1.2g / hr, and the flow rate of the main catalyst is 0.36g / hr. The prepolymerization is carried out in a bulk propylene liquid phase environment, the temperature is 15°C, and the residence time is about 4 minutes.
[0148] After the prepolymerization, the catalyst continuously enters the loop reactor to complete the propylene homopolymerization reaction in the loop reactor. The loop polymerization reaction temperature is 70° C., the reaction pressure is 4.0 MPa, and hydrogen is added to the feed of the loop reactor. The hydrogen concentration detected by online chromatography is 0.15 mol%. Accordingly, the hydrogen / propylene ratio is 0.0015 mol / mol.
[0149] After the reaction in the loop reactor, the obtained material enters the fluidized bed gas phase reactor for copolymerization of ethylene and propylene. The gas phase reaction temperature is 70°C, the reaction pressure is 1.1 MPa, wherein ethylene / (propylene+ethylene)=0.21 (mol / mol), a certain amount of hydrogen is added to the feed of the gas phase reactor, and the hydrogen / ethylene in the circulating gas of the gas phase reactor is detected by online chromatography=0.13 (mol / mol). The specific process conditions are shown in Table 1.
[0150] The polymer obtained by the reaction is subjected to degassing and wet nitrogen deactivation treatment to obtain a polypropylene composition.
[0151] The ethylene content of component B in the obtained polypropylene composition was 31.0 wt%, and the ratio of MFR of component A to MFR of the composition was 1.08.
[0152] (2) Preparation of polypropylene pellets and injection molded samples
[0153] 0.1 wt% of IRGAFOS 168 (BASF, Germany), 0.1 wt% of IRGANOX 1010 (BASF, Germany), 0.05 wt% of calcium stearate and 0.04 wt% of Millad HPN-20E nucleating agent (Milliken & Company, USA) were added to the polypropylene composition obtained by polymerization, and pelletized using a twin-screw extruder. Then, an injection molding machine was used to prepare injection molding samples that met the GB standard, and their physical properties were measured.
[0154] The measurement results are shown in Table 2.
[0155] Figure 1-Figure 3The SEM photos of the pellets and injection molded samples prepared in Example A1 are shown. From these SEM photos, it can be seen that after injection molding, the rubber phase in the injection molded sample of Example A1 presents an obvious oriented structure. Regardless of the position within the 10% thickness range from the product surface and the position of the core part outside the 10% thickness range from the product surface, the rubber phase is deformed, elongated and oriented along a certain direction, and the deformation degree of the rubber phase within the 10% thickness range from the product surface is higher (the position within the 10% thickness range from the product surface: more than 70% of the rubber phase particles have an aspect ratio greater than 4, and some rubber phase particles have an aspect ratio greater than 7; the core part position outside the 10% thickness range from the product surface: more than 50% of the rubber phase particles have an aspect ratio greater than 2). In addition, it can also be seen that the rubber phase in the pellets before injection molding is basically spherical. Therefore, the orientation force applied during the injection molding process causes the rubber phase to deform and form an oriented structure, and after the orientation force is removed and the sample is formed, the rubber phase maintains the oriented structure.
[0156] Example A2
[0157] The catalyst system, nucleating agent and polymerization process conditions used in Example A2 are the same as those in Example A1, but the difference from Example A1 is that the hydrogen concentration in the loop reactor is 0.21 mol%, and the hydrogen / ethylene ratio in the gas phase reactor is 0.1 (mol / mol). The specific process conditions are shown in Table 1. The ethylene content in component B in the obtained polypropylene composition is 31.1% by weight, and the ratio of the MFR of component A to the MFR of the composition is 1.28.
[0158] The performance test results of the obtained injection molded samples are shown in Table 2.
[0159] SEM analysis shows that after injection molding, the rubber phase in the injection-molded sample of Example A2 presents a distinct oriented structure.
[0160] Example A3
[0161] The catalyst system, nucleating agent and polymerization process conditions used in Example A3 are the same as those in Example A1, but the difference from Example A1 is that hydrogen / ethylene in the gas phase reactor = 0.14 (mol / mol), ethylene / (ethylene+propylene) = 0.25 (mol / mol). The specific process conditions are shown in Table 1. The ethylene content in component B in the obtained polypropylene composition is 34.89% by weight, and the ratio of the MFR of component A to the MFR of the composition is 0.93.
[0162] The performance test results of the obtained injection molded samples are shown in Table 2.
[0163] SEM analysis shows that after injection molding, the rubber phase in the injection-molded sample of Example A3 presents a distinct oriented structure.
[0164] Example A4
[0165] The catalyst system, nucleating agent and polymerization process conditions used in Example A4 are the same as those in Example A1, but the difference from Example A1 is that the hydrogen concentration in the loop reactor is 0.23 mol%, and the hydrogen / ethylene ratio in the gas phase reactor is 0.02 (mol / mol). The specific process conditions are shown in Table 1. The ethylene content in component B in the obtained polypropylene composition is 31.2% by weight, and the ratio of the MFR of component A to the MFR of the composition is 1.81.
[0166] The performance test results of the obtained injection molded samples are shown in Table 2.
[0167] SEM analysis shows that after injection molding, the rubber phase in the injection-molded sample of Example A4 presents a distinct oriented structure.
[0168] Example A5
[0169] The catalyst system, nucleating agent and polymerization process conditions used in Example A5 are the same as those in Example A1, but the difference from Example A1 is that the hydrogen concentration in the loop reactor is 0.26 mol%, and in the gas phase reactor, ethylene / (propylene+ethylene)=0.19 (mol / mol), hydrogen / ethylene=0.35 (mol / mol). The specific process conditions are shown in Table 1.
[0170] The ethylene content of component B in the obtained polypropylene composition was 30.96 wt%, and the ratio of MFR of component A to MFR of the composition was 1.14.
[0171] The performance test results of the obtained injection molded samples are shown in Table 2.
[0172] SEM analysis showed that after injection molding, the rubber phase in the injection-molded sample of Example A5 exhibited a distinct oriented structure.
[0173] Example A6
[0174] The catalyst system, nucleating agent and polymerization process conditions used in Example A6 are the same as those in Example A1, but the difference from Example A1 is that the hydrogen concentration in the loop reactor is 0.60 mol%, and in the gas phase reactor, hydrogen / ethylene=0.04 (mol / mol). The specific process conditions are shown in Table 1.
[0175] The ethylene content of component B in the obtained polypropylene composition was 31.67 wt%, and the ratio of MFR of component A to MFR of the composition was 1.85.
[0176] The performance test results of the obtained injection molded samples are shown in Table 2.
[0177] SEM analysis showed that after injection molding, the rubber phase in the injection-molded sample of Example A6 exhibited a distinct oriented structure.
[0178] Comparative Example A1
[0179] The catalyst system, nucleating agent and polymerization process conditions used in Comparative Example A1 are the same as those in Example A1, but the difference from Example A1 is that the hydrogen concentration in the loop reactor is 0.28 mol%, and in the gas phase reactor, ethylene / (propylene+ethylene)=0.45 (mol / mol), hydrogen / ethylene=0.01 (mol / mol). The specific process conditions are shown in Table 1.
[0180] The ethylene content of component B in the obtained polypropylene composition was 48.61 wt%, and the ratio of MFR of component A to MFR of the composition was 2.49.
[0181] The performance test results of the obtained injection molded samples are shown in Table 2.
[0182] Comparative Example A2
[0183] The catalyst system, nucleating agent and polymerization process conditions used in Comparative Example A2 are the same as those in Example A1, but the difference from Example A1 is that the hydrogen concentration in the loop reactor is 0.70 mol%, and in the gas phase reactor, ethylene / (propylene+ethylene)=0.45 (mol / mol), hydrogen / ethylene=0.02 (mol / mol). The specific process conditions are shown in Table 1.
[0184] The ethylene content of component B in the obtained polypropylene composition was 48.58 wt%, and the ratio of MFR of component A to MFR of the composition was 2.34.
[0185] The performance test results of the obtained injection molded samples are shown in Table 2.
[0186] Figure 6 and Figure 7 SEM photos of the injection molded sample and pellets of Comparative Example A2 are shown. From these photos, it can be seen that even after injection molding, the rubber phase in the injection molded sample of Comparative Example A2 is still basically spherical, without deformation and orientation, especially at the core part outside the range of 10% thickness from the surface of the product, where no deformation and orientation tendency can be seen.
[0187]
[0188]
[0189] It can be seen from the data in Tables 1 and 2 that the polypropylene composition of the present invention has higher gloss and comparable or better mechanical properties than when the polymerization process conditions are adjusted so that the ethylene content in the ethylene-propylene elastomeric copolymer and / or the ratio of the melt mass flow rate of the homopolypropylene and the polypropylene composition are not within the scope of the present invention.
[0190] Thus, the polypropylene composition of the present invention can be used in particular for the preparation of articles combining good mechanical properties (high stiffness, high toughness and low shrinkage properties) with aesthetic properties (high gloss).
[0191] Example B1
[0192] Preparation of main catalyst Cat-1: In a 300mL glass reaction bottle, add 90mL (820mmol) of titanium tetrachloride and cool to -20°C, add 37mmol of magnesium halide carrier (prepared according to the method disclosed in Example 1 of CN1330086A) in terms of magnesium element, then heat to 110°C, and add 0.3mmol of tributyl phosphate and 7.3mmol of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane during the heating process. After maintaining at 110°C for 30min, filter out the liquid, wash twice with titanium tetrachloride, wash five times with hexane, and obtain catalyst component Cat-1 after vacuum drying.
[0193] The phosphorus content of the catalyst component Cat-1 was measured by X-ray fluorescence spectrometry (X-ray fluorescence spectrometer: PANalytical, Netherlands, model: Zetium) to be 0.011 wt % in terms of phosphorus element.
[0194] The polymerization reaction was carried out on a polypropylene pilot plant. The polymerization method and steps are as follows:
[0195] Prepolymerization: The main catalyst Cat-1, the cocatalyst (triethylaluminum), and the external electron donor methylcyclohexyldimethoxysilane (CHMMS) were pre-contacted at 10°C for 20 minutes and then continuously added to the prepolymerization reactor for prepolymerization. The flow rate of triethylaluminum (TEAL) was 6 g / hr, the flow rate of methylcyclohexyldimethoxysilane was 1.2 g / hr, and the flow rate of the main catalyst was 0.36 g / hr. The prepolymerization was carried out in a bulk propylene liquid phase environment at a temperature of 15°C and a residence time of about 4 minutes.
[0196] After prepolymerization, the catalyst continuously enters the loop reactor to complete propylene homopolymerization in the loop reactor. The loop polymerization temperature is 70° C., the reaction pressure is 4.0 MPa, hydrogen is added to the feed of the loop reactor, and the hydrogen concentration detected by online chromatography is 0.10 mol%.
[0197] After the reaction in the loop reactor, the obtained material enters the fluidized bed gas phase reactor for copolymerization of ethylene and propylene. The gas phase reaction temperature is 70°C, the reaction pressure is 1.1 MPa, wherein ethylene / (propylene+ethylene)=0.21 (volume ratio), a certain amount of hydrogen is added to the feed of the gas phase reactor, and the hydrogen / ethylene in the circulating gas of the gas phase reactor is detected by online chromatography=0.11. The specific process is shown in Table 3.
[0198] The ethylene content of component B in the obtained polypropylene composition was 28.04 wt%, and the ratio of MFR of component A to MFR of the composition was 0.87.
[0199] The polymer obtained by the reaction is degassed and deactivated with wet nitrogen to obtain polymer powder.
[0200] 0.1 wt% IRGAFOS 168, 0.1 wt% IRGANOX 1010, 0.05 wt% calcium stearate, 0.05 wt% Millad HPN-715 and 0.05 wt% Millad600EI nucleating agent were added to the powder obtained by polymerization, and granulated by a twin-screw extruder to obtain polypropylene composition pellets. Then, an injection molding machine was used to prepare injection molding samples that met the GB standard, and their physical properties were measured. The measurement results are shown in Table 4.
[0201] Figure 4 The SEM photograph of the injection-molded sample of Example B1 shows the core portion located outside the 10% thickness range from the surface of the product. Figure 5 SEM photos of the pellets of Example B1 are shown. From these SEM photos, it can be seen that after injection molding, the rubber phase in the injection molded sample prepared by Example B1 presents a clear oriented structure, and the rubber phase is also deformed and oriented at the core part outside the 10% thickness range from the product surface (at the core part outside the 10% thickness range from the product surface: more than 70% of the rubber phase particles have an aspect ratio greater than 2, and some rubber phase particles even have an aspect ratio greater than 4); while the rubber phase in the pellets before injection molding is basically spherical.
[0202] Example B2
[0203] The catalyst system, nucleating agent and polymerization process conditions used in Example B2 are the same as those in Example B1, but the difference from Example B1 is that the hydrogen concentration in the loop reactor is 0.13 mol%, and the hydrogen / ethylene in the gas phase reactor is 0.08 (mol / mol). The specific process conditions are shown in Table 3.
[0204] The ethylene content of component B in the obtained polypropylene composition was 28.05 wt%, and the ratio of MFR of component A to MFR of the composition was 1.27.
[0205] The performance test results of the obtained injection molded samples are shown in Table 4.
[0206] SEM analysis showed that after injection molding, the rubber phase in the injection-molded sample of Example B2 exhibited a distinct oriented structure.
[0207] Example B3
[0208] The catalyst system, nucleating agent and polymerization process conditions used in Example B3 are the same as those in Example B1, but the difference from Example B1 is that ethylene / (propylene+ethylene) in the gas phase reactor is 0.25 (mol / mol), and hydrogen / ethylene is 0.12 (mol / mol). The specific process conditions are shown in Table 3.
[0209] The ethylene content of component B in the obtained polypropylene composition was 33.67 wt%, and the ratio of MFR of component A to MFR of the composition was 0.93.
[0210] The performance test results of the obtained injection molded samples are shown in Table 4.
[0211] SEM analysis showed that after injection molding, the rubber phase in the injection-molded sample of Example B3 exhibited a distinct oriented structure.
[0212] Example B4
[0213] The catalyst system, nucleating agent and polymerization process conditions used in Example B4 are the same as those in Example B1, but the difference from Example B1 is that the hydrogen concentration in the loop reactor is 0.13 mol%, the ethylene / (propylene+ethylene) in the gas phase reactor is 0.15 (mol / mol), and the hydrogen / ethylene is 0.18 (mol / mol). The specific process conditions are shown in Table 3.
[0214] The ethylene content of component B in the obtained polypropylene composition was 26.72 wt%, and the ratio of MFR of component A to MFR of the composition was 1.04.
[0215] The performance test results of the obtained injection molded samples are shown in Table 4.
[0216] SEM analysis showed that after injection molding, the rubber phase in the injection-molded sample of Example B4 exhibited a distinct oriented structure.
[0217] Example B5
[0218] The catalyst system, nucleating agent and polymerization process conditions used in Example B5 are the same as those in Example B1, but the difference from Example B1 is that the hydrogen concentration in the loop reactor is 0.18 mol%, the ethylene / (propylene+ethylene) in the gas phase reactor is 0.19 (mol / mol), and the hydrogen / ethylene is 0.22 (mol / mol). The specific process conditions are shown in Table 3.
[0219] The ethylene content of component B in the obtained polypropylene composition was 27.89 wt%, and the ratio of MFR of component A to MFR of the composition was 1.09.
[0220] The performance test results of the obtained injection molded samples are shown in Table 4.
[0221] SEM analysis showed that after injection molding, the rubber phase in the injection-molded sample of Example B5 exhibited a distinct oriented structure.
[0222] Example B6
[0223] The catalyst system, nucleating agent and polymerization process conditions used in Example B6 are the same as those in Example B1, but the difference from Example B1 is that the hydrogen concentration in the loop reactor is 0.24 mol%, the ethylene / (propylene+ethylene) in the gas phase reactor is 0.13 (mol / mol), and the hydrogen / ethylene is 0.54 (mol / mol). The specific process conditions are shown in Table 3.
[0224] The ethylene content of component B in the obtained polypropylene composition was 25.05 wt%, and the ratio of MFR of component A to MFR of the composition was 1.04.
[0225] The performance test results of the obtained injection molded samples are shown in Table 4.
[0226] SEM analysis showed that after injection molding, the rubber phase in the injection-molded sample of Example B6 exhibited a distinct oriented structure.
[0227] Example B7
[0228] The catalyst system, nucleating agent and polymerization process conditions used in Example B7 are the same as those in Example B1, but the difference from Example B1 is that the hydrogen concentration in the loop reactor is 0.35 mol%, the ethylene / (propylene+ethylene) in the gas phase reactor is 0.21 (mol / mol), and the hydrogen / ethylene is 0.10 (mol / mol). The specific process conditions are shown in Table 3.
[0229] The ethylene content of component B in the obtained polypropylene composition was 28.05 wt%, and the ratio of MFR of component A to MFR of the composition was 1.53.
[0230] The performance test results of the obtained injection molded samples are shown in Table 4.
[0231] SEM analysis showed that after injection molding, the rubber phase in the injection-molded sample of Example B7 exhibited a distinct oriented structure.
[0232] Example C1
[0233] The internal electron donor of the main catalyst used in Example C1 is diisobutyl phthalate, and the external electron donor, cocatalyst, nucleating agent and polymerization process conditions are the same as those of Example B5, but the difference from Example B5 is that the hydrogen concentration in the loop reactor is 0.24 mol%, and the hydrogen / ethylene in the gas phase reactor is 0.35 (mol / mol). The specific process conditions are shown in Table 3.
[0234] The ethylene content of component B in the obtained polypropylene composition was 30.98 wt%, and the ratio of MFR of component A to MFR of the composition was 1.08.
[0235] The performance test results of the obtained injection molded samples are shown in Table 4.
[0236] Example C2
[0237] The internal electron donors of the main catalyst used in Example C2 are diisobutyl phthalate and diethyl phthalate, and the external electron donor, cocatalyst and polymerization process conditions are the same as those of Example B1, but the difference from Example B1 is that no nucleating agent is added. The specific process conditions are shown in Table 3.
[0238] The ethylene content of component B in the obtained polypropylene composition was 28.04 wt%, and the ratio of MFR of component A to MFR of the composition was 0.87.
[0239] The performance test results of the obtained injection molded samples are shown in Table 4.
[0240] Comparative Example C1
[0241] The internal electron donor of the main catalyst used in Comparative Example C1 is diisobutyl phthalate, the external electron donor is diisopropyldimethoxysilane (DIPMS), and the cocatalyst, nucleating agent and polymerization process conditions are the same as those of Example B1. The difference from the process conditions of Example B1 is that the hydrogen concentration in the loop reactor is 0.25 mol%, and in the gas phase reactor, ethylene / (propylene+ethylene)=0.45 (mol / mol), hydrogen / ethylene=0.02 (mol / mol). The specific process conditions are shown in Table 3.
[0242] The ethylene content of component B in the obtained polypropylene composition was 48.61 wt%, and the ratio of MFR of component A to MFR of the composition was 2.03.
[0243] The performance test results of the obtained injection molded samples are shown in Table 4.
[0244] Comparative Example C2
[0245] The internal electron donor of the main catalyst used in Comparative Example C2 is diisobutyl phthalate, the external electron donor is diisopropyldimethoxysilane (DIPMS), the cocatalyst, the nucleating agent and the polymerization process conditions are the same as those in Example B1, but the difference from the process conditions in Example B1 is that the hydrogen concentration in the loop reactor is 0.65 mol%, and in the gas phase reactor, ethylene / (propylene+ethylene)=0.45 (mol / mol), hydrogen / ethylene=0.02 (mol / mol). The specific process conditions are shown in Table 3.
[0246] The ethylene content of component B in the obtained polypropylene composition was 48.58 wt%, and the ratio of MFR of component A to MFR of the composition was 1.95.
[0247] The performance test results of the obtained injection molded samples are shown in Table 4.
[0248] Comparative Example C3
[0249] The internal electron donor of the main catalyst used in Comparative Example C3 is diisobutyl phthalate, and the external electron donor, cocatalyst, nucleating agent and polymerization process conditions are the same as those of Example B5, but the difference from Example B5 is that the hydrogen concentration in the loop reactor is 0.18 mol%, and the hydrogen / ethylene in the gas phase reactor is 0.35 (mol / mol). The specific process conditions are shown in Table 3.
[0250] The ethylene content of component B in the obtained polypropylene composition was 31.05 wt%, and the ratio of MFR of component A to MFR of the composition was 1.05.
[0251] The performance test results of the obtained injection molded samples are shown in Table 4.
[0252]
[0253]
[0254]
[0255] It can be seen from the data in Tables 3 and 4 that, compared with the case where the polymerization process conditions are adjusted so that the regularity of the homopolypropylene, the ethylene content in the ethylene-propylene elastic copolymer and / or the ratio of the melt mass flow rate of the homopolypropylene and the polypropylene composition are not within the scope of the present invention, the polypropylene composition of the present invention has lower haze and higher gloss, and thus has better transparency and aesthetic properties; at the same time, it has equivalent or better mechanical properties.
[0256] Compared with a catalyst system using carboxylic acid ester as an internal electron donor, a polypropylene composition prepared by a catalyst system using a phosphate compound and a diether compound as an internal electron donor has higher gloss and lower haze and has comparable mechanical properties, and can have good transparency, high gloss, high rigidity, high toughness and low shrinkage properties, thereby having both good mechanical properties and aesthetic characteristics.
[0257] In addition, by comparing Example C2 with Example B1, it can be seen that a nucleating agent is added to Example B1, so that the modulus of the obtained product is higher and the haze is lower.
[0258] The present invention has been described above by way of example in conjunction with the embodiments, but the descriptions shown are not exhaustive and are not intended to limit the scope of the present invention. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the present invention.
[0259] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A polypropylene composition comprising: (a) 70-95 wt% of a crystalline homopolymer polypropylene as component A, wherein the isotactic pentad fraction is greater than 97%; the crystalline homopolymer polypropylene forms a continuous matrix phase in the polypropylene composition; (b) 5-30 wt% of an ethylene-propylene elastic copolymer as component B, wherein the ethylene-propylene elastic copolymer contains 20-35 wt% of ethylene structural units and 65-80 wt% of propylene structural units, based on the total weight of the ethylene-propylene elastic copolymer; the ethylene-propylene elastic copolymer forms a dispersed rubber phase in the continuous matrix phase, and the rubber phase can be at least partially deformed under the action of the orientation force and form an oriented structure; wherein the ratio of the melt mass flow rate of the crystalline homopolypropylene to the melt mass flow rate of the polypropylene composition measured at 230° C. and 2.16 kg load according to GB / T 3682.1-2018 is 0.5-2.0; The crystalline homopolypropylene has a melt mass flow rate of 10-100 g / 10 min at 230° C. and a load of 2.16 kg according to GB / T 3682.1-2018.
2. The polypropylene composition according to claim 1, wherein the ethylene-propylene elastomeric copolymer contains 25-35 wt% of ethylene structural units and 65-75 wt% of propylene structural units, based on the total weight of the ethylene-propylene elastomeric copolymer.
3. The polypropylene composition according to claim 1, wherein a ratio of the melt mass flow rate of the crystalline homopolypropylene to that of the polypropylene composition measured at 230°C and a load of 2.16 kg according to GB / T 3682.1-2018 is 0.9-1.
5.
4. The polypropylene composition according to claim 1, wherein when no orientation force is applied, the rubber phase is in the form of spherical or nearly spherical particles and the average size of the rubber phase particles is 0.03-3.0 μm, as measured by SEM method.
5. The polypropylene composition according to claim 1, wherein when no orientation force is applied, the average size of the rubber phase particles is 0.05-2.0 μm, as measured by SEM method.
6. The polypropylene composition according to claim 1, wherein when no orientation force is applied, the average size of the rubber phase particles is 0.05-1.5 μm, as measured by SEM method.
7. The polypropylene composition of claim 1, wherein after the orientation force is applied, at least 50% of the rubber phase particles have an aspect ratio greater than 2, based on the total number of rubber phase particles in the SEM photograph.
8. The polypropylene composition according to claim 1, wherein the orientation force refers to an external field force that can cause an object to be oriented, and the orientation refers to the parallel arrangement of the object along the direction of the external field force; the oriented state structure refers to the longitudinal axes formed by the deformation and elongation of rubber phase particles under the action of the orientation force and arranged parallel to each other along a certain direction.
9. The polypropylene composition according to claim 8, wherein the orienting force is a tensile stress and / or a shear stress.
10. The polypropylene composition according to claim 8, wherein the orientation forces are forces exerted on the polypropylene composition by the process itself for preparing the article.
11. The polypropylene composition of claim 8, wherein under the action of the orientation force, at least 80% of the rubber phase particles form an oriented structure based on the total number of rubber phase particles in the SEM image.
12. The polypropylene composition according to claim 1, wherein the polypropylene composition has a melt mass flow rate of 5-100 g / 10 min at 230°C and a load of 2.16 kg according to GB / T 3682.1-2018.
13. The polypropylene composition according to claim 12, wherein the polypropylene composition has a melt mass flow rate of 6-30 g / 10 min at 230°C and a load of 2.16 kg according to GB / T 3682.1-2018.
14. The polypropylene composition according to claim 12, wherein the polypropylene composition has a melt mass flow rate of 8.89-30 g / 10 min at 230°C and a load of 2.16 kg according to GB / T 3682.1-2018.
15. The polypropylene composition according to claim 1, wherein the intrinsic viscosity of the polypropylene composition is 1.0-2.5 dL / g; and / or, The xylene solubles in the polypropylene composition have an intrinsic viscosity of 1.0-4.0 dL / g; and / or, The ratio of the intrinsic viscosity of xylene soluble matter in the polypropylene composition to the intrinsic viscosity of the crystalline homopolymer polypropylene is 0.7-2.
6.
16. The polypropylene composition according to claim 15, wherein the polypropylene composition has an intrinsic viscosity of 1.4 to 2.4 dL / g.
17. The polypropylene composition according to claim 15, wherein the polypropylene composition has an intrinsic viscosity of 1.52 to 2.08 dL / g.
18. The polypropylene composition according to claim 15, wherein the intrinsic viscosity of xylene solubles in the polypropylene composition is 1.11-3.65 dL / g.
19. The polypropylene composition of claim 1, wherein the polypropylene composition has a molecular weight distribution Mw / Mn ≤ 5 as measured by gel permeation chromatography (GPC) analysis relative to polystyrene standards.
20. The polypropylene composition according to claim 19, wherein the polypropylene composition has a molecular weight distribution Mw / Mn≤4.5 as measured by gel permeation chromatography (GPC) analysis relative to polystyrene standards.
21. The polypropylene composition according to claim 1, wherein the gloss at 60° angle of the polypropylene composition is ≥ 80%.
22. The polypropylene composition according to claim 21, wherein the gloss at 60° angle of the polypropylene composition is ≥ 85%.
23. The polypropylene composition according to claim 21, wherein the gloss at 60° angle of the polypropylene composition is ≥ 90%.
24. The polypropylene composition of claim 21, wherein the polypropylene composition has a haze of ≤ 50%.
25. The polypropylene composition of claim 21, wherein the polypropylene composition has a haze of ≤ 40%.
26. The polypropylene composition according to any one of claims 21 to 25, wherein the polypropylene composition additionally has one or more of the following properties: 1) Parallel shrinkage ratio ≤1.15; 2) Vertical shrinkage ratio ≤1.36; 3) Flexural modulus ≥ 1000MPa; 4) Room temperature simply supported beam notched impact strength ≥5kJ / m 2 ; 5) Heat deformation temperature ≥90℃.
27. Polypropylene composition according to claim 26, wherein the polypropylene composition additionally has all of the mentioned properties.
28. The polypropylene composition according to claim 26, wherein the parallel shrinkage ratio is ≤ 1.
1.
29. The polypropylene composition according to claim 26, wherein the vertical shrinkage ratio is ≤ 1.
15.
30. The polypropylene composition according to claim 26, wherein the flexural modulus is > 1300 MPa.
31. The polypropylene composition according to claim 26, wherein the flexural modulus is ≥ 1400 MPa.
32. The polypropylene composition of claim 26, wherein the flexural modulus is > 1450 MPa.
33. The polypropylene composition according to claim 26, wherein the room temperature simple supported beam notched impact strength is ≥ 6 kJ / m 2 .
34. The polypropylene composition of claim 26, wherein the heat distortion temperature is ≥ 92°C.
35. The polypropylene composition according to claim 1, wherein the polypropylene composition further comprises: (c) a nucleating agent as component C.
36. The polypropylene composition according to claim 35, wherein the nucleating agent is at least one selected from carboxylic acids and metal salts thereof, sorbitols, aromatic phosphates, dehydroabietic acid and salts thereof, aromatic amides, aromatic amines, rare earth compounds, condensed ring compounds having a quasi-planar structure, and polymer nucleating agents.
37. The polypropylene composition according to claim 35, wherein the nucleating agent is present in an amount of 0.05-0.3 wt%, based on the total weight of the polypropylene composition.
38. The polypropylene composition according to claim 1 or 35, wherein the polypropylene composition further comprises other additives, and the other additives are selected from at least one of antioxidants, antistatic agents and colorants.
39. The polypropylene composition according to claim 38, wherein the content of the other auxiliary agent is 0.05-0.6 wt% based on the total weight of the polypropylene composition.
40. The polypropylene composition according to claim 38, wherein the content of the other auxiliary agent is 0.1-0.3 wt% based on the total weight of the polypropylene composition.
41. The polypropylene composition according to claim 1, wherein the polypropylene composition is in the form of powder or pellets.
42. A method for preparing a polypropylene composition according to any one of claims 1 to 41, comprising the following steps: (1) contacting a propylene monomer with a stereoselective Ziegler-Natta catalyst under a first olefin polymerization condition, and removing unreacted monomers from a mixture obtained after the contact reaction to obtain a product a, wherein the product a comprises component A; (2) under the second olefin polymerization conditions, in the gas phase, ethylene monomer and propylene monomer are contacted with the product a obtained in step (1) for reaction, and unreacted monomers are removed from the mixture obtained after the contact reaction to obtain a product b comprising component A and component B as the polypropylene composition.
43. The process of claim 42, wherein the stereoselective Ziegler-Natta catalyst comprises: (i) a solid catalyst component, the solid catalyst component comprising a product obtained by reacting a magnesium source, a titanium source and an internal electron donor; (ii) organoaluminium compounds; and (iii) an optional external electron donor.
44. The method of claim 43, wherein the internal electron donor is selected from the group consisting of esters of monocarboxylic acids, esters of dicarboxylic acids, phosphate compounds, and diether compounds, and combinations thereof.
45. The method of claim 43, wherein The magnesium source is selected from magnesium halide, magnesium alcoholate or halogenated alcoholate and magnesium halide adduct carrier; The titanium source is selected from the general formula Ti(OR) 4-m X m One or more of the titanium compounds shown, wherein m is an integer of 0-4, and R is C1-C 20 wherein X is halogen.
46. The method of claim 45, wherein the magnesium source is a spherical magnesium halide adduct.
47. The method of claim 45, wherein m is an integer from 1 to 4.
48. The method of claim 45, wherein R is C1-C 10 of alkyl.
49. The method of claim 45, wherein X is chlorine.
50. The method of claim 43, wherein the organoaluminum compound is an alkylaluminum compound.
51. The method according to claim 43, wherein the organoaluminum compound is at least one of triethylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-hexylaluminum, diethylaluminum monochloride, di-n-butylaluminum monochloride, diisobutylaluminum monochloride, di-n-hexylaluminum monochloride, monoethylaluminum dichloride, mono-n-butylaluminum dichloride, monoisobutylaluminum dichloride and mono-n-hexylaluminum dichloride.
52. The method of claim 43, wherein the external electron donor is an organosilicon compound.
53. The method according to claim 52, wherein the organosilicon compound is of the general formula R n Si(OR') 4-n An organosilicon compound, wherein 0<n≤3, R is selected from hydrogen atom, halogen, alkyl, cycloalkyl, aryl and halogenated alkyl, and R' is selected from alkyl, cycloalkyl, aryl and halogenated alkyl.
54. The method according to claim 52, wherein the external electron donor is selected from at least one of tetramethoxysilane, tetraethoxysilane, trimethylmethoxysilane, trimethylethoxysilane, trimethylphenoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methyl-tert-butyldimethoxysilane, methylisopropyldimethoxysilane, diphenoxydimethoxysilane, diphenyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, cyclohexylmethyldimethoxysilane, dicyclopentyldimethoxysilane, diisopropyldimethoxysilane, diisobutyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane.
55. The method of claim 43, wherein the catalyst is pre-complexed and / or pre-polymerized.
56. The method of claim 44, wherein the internal electron donor is selected from at least one of benzoates, malonates, phthalates, and succinates.
57. The method of claim 56, wherein the internal electron donor is an alkyl phthalate.
58. The method of claim 56, wherein the internal electron donor is diisobutyl phthalate and / or dioctyl phthalate.
59. The method according to claim 43, wherein the internal electron donor is an internal electron donor composed of a phosphate compound and a diether compound.
60. The method according to claim 59, wherein the molar ratio of the diether compound to the phosphate ester compound is 1:(0.02-0.25).
61. The method according to claim 59, wherein the molar ratio of the diether compound to the phosphate compound is 1:(0.04-0.15).
62. The method according to claim 59, wherein the phosphate compound is selected from at least one of the phosphate compounds represented by formula (1), in, R1, R2 and R3 are each independently selected from a C1-C4 straight chain or branched alkyl group, a C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkyl or C7-C 20 of aralkyl.
63. The method of claim 59, wherein the phosphate compound is selected from at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate, triphenyl phosphate, tricresyl phosphate, triisopropylphenyl phosphate, trimethoxyphenyl phosphate, phenyl dimethyl phosphate, cresyl dibutyl phosphate, isopropylphenyl dimethyl phosphate, isopropylphenyl diethyl phosphate, isopropylphenyl dibutyl phosphate, phenyl xylyl phosphate, phenyl diisopropylphenyl phosphate, p-cresyl dibutyl phosphate, m-cresyl dibutyl phosphate, p-cumyl dimethyl phosphate, p-cumyl diethyl phosphate, p-tert-butylphenyl dimethyl phosphate and o-cresyl p-di-tert-butylphenyl phosphate.
64. The method according to claim 59, wherein the diether compound is selected from at least one of the diether compounds represented by formula (2), R 1 R 2 C(CH2OR 3 )(CH2OR 4 ) Formula (2) in, R 1 and R 2 Each independently selected from hydrogen, C1-C 20 Straight or branched alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Arylalkyl or C7-C 20 Alkyl, R 3 and R 4 Each independently selected from C1-C 10 of alkyl.
65. The method of claim 59, wherein The diether compound is selected from 2-(2-ethylhexyl)-1,3-dimethoxypropane, 2-isopropyl-1,3-dimethoxypropane, 2-butyl-1,3-dimethoxypropane, 2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-1,3-dimethoxypropane, 2-phenyl-1,3-dimethoxypropane, 2-(2-phenylethyl)-1,3-dimethoxypropane, 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-(p-chlorophenyl)-1,3-dimethoxypropane, 2-(diphenylmethyl)-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, 2,2- Dicyclopentyl-1,3-dimethoxypropane, 2,2-diethyl-1,3-dimethoxypropane, 2,2-dipropyl-1,3-dimethoxypropane, 2,2-diisopropyl-1,3-dimethoxypropane, 2,2-dibutyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-benzyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-phenyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane, 2,2-bis( 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-diphenyl-1,3-dimethoxypropane, 2,2-dibenzyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2-isobutyl-2-isopropyl-1,3-dimethoxypropane, 2-(1-methylbutyl)-2-isopropyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, 2 -phenyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2-sec-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclohexyl-2-sec-butyl-1,3-dimethoxypropane, 2-isopropyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane and at least one of 9,9-dimethoxymethylfluorene.
66. The method according to claim 43, wherein the molar ratio of the magnesium source calculated as magnesium element, the titanium source calculated as titanium element and the internal electron donor is 1:(20-150):(0.1-0.9); and / or, The solid catalyst component and the organoaluminum compound are used in a titanium / aluminum molar ratio of 1:(25-100); and / or, The weight ratio of the organic aluminum compound to the external electron donor is (0-150):
1.
67. The method according to claim 66, wherein the molar ratio of the magnesium source calculated as magnesium element, the titanium source calculated as titanium element and the internal electron donor is 1:(30-120):(0.15-0.6).
68. The method of claim 66, wherein the weight ratio of the organoaluminum compound to the external electron donor is (2-150):
1.
69. The method of claim 66, wherein the weight ratio of the organoaluminum compound to the external electron donor is (3-10):
1.
70. The method according to claim 42, wherein the first olefin polymerization conditions in step (1) are liquid phase polymerization conditions or gas phase polymerization conditions; the liquid phase polymerization conditions include: Hydrogen is used as a molecular weight regulator and the polymerization temperature is 0-150°C; The polymerization pressure is higher than the saturated vapor pressure of propylene at the corresponding polymerization temperature; The gas phase polymerization conditions include: using hydrogen as a molecular weight regulator, a polymerization temperature of 0-150° C., and a polymerization pressure greater than or equal to normal pressure.
71. The process of claim 70, wherein the polymerization temperature is 40-100°C in liquid phase polymerization conditions.
72. The process of claim 70, wherein the polymerization temperature is 40-100°C in gas phase polymerization conditions.
73. The method of claim 70, wherein in the gas phase polymerization condition, the polymerization pressure is 0.5-2.5 MPa.
74. The method of claim 42, wherein the hydrogen / propylene ratio used in step (1) is 0.0010-0.0060 mol / mol.
75. The method according to claim 42, wherein in the reaction system of step (2), The molar ratio of ethylene / (ethylene+propylene) is 0.1-0.4 mol / mol; and / or, The temperature of the olefin gas phase polymerization is 40-100°C; and the pressure is 0.6-1.4 MPa; and / or, The hydrogen / ethylene ratio is 0.02-0.70 mol / mol.
76. The method according to claim 75, wherein in the reaction system of step (2), the molar ratio of ethylene / (ethylene+propylene) is 0.1-0.3 mol / mol.
77. The method according to claim 75, wherein in the reaction system of step (2), the molar ratio of ethylene / (ethylene+propylene) is 0.15-0.25 mol / mol.
78. The method according to claim 75, wherein in the reaction system of step (2), the temperature of olefin gas phase polymerization is 60-80°C.
79. The method according to claim 75, wherein in the reaction system of step (2), the pressure of olefin gas phase polymerization is 1.0-1.3 MPa.
80. The method according to claim 75, wherein in the reaction system of step (2), the hydrogen / ethylene ratio is 0.04-0.54 mol / mol.
81. The method according to any one of claims 42 to 80, wherein the method further comprises step (3): mixing the product b obtained in step (2) with a nucleating agent and optionally other auxiliary agents.
82. The method according to claim 81, wherein in step (3), granulation is further performed.
83. An article prepared from the polypropylene composition according to any one of claims 1 to 41, wherein at least a portion of the rubber phase particles in the rubber phase are deformed and form an oriented structure.
84. The article of claim 83, wherein the article is an injection molded article.
85. The article of claim 83, wherein at least 80% of the rubber phase particles in the rubber phase are deformed and form an oriented structure.
86. The article according to claim 83, wherein the rubber phase at a position within 10% thickness range from the surface of the article and at a core portion outside the 10% thickness range from the surface of the article is deformed and elongated to form an oriented structure.
87. The article of claim 83, wherein more than 50% of the rubber phase particles within 10% thickness from the surface of the article have an aspect ratio greater than or equal to 4; and more than 50% of the rubber phase particles in the core portion outside the 10% thickness range from the surface of the article have an aspect ratio greater than or equal to 2, based on the total number of rubber phase particles in the SEM photograph at the corresponding position.
88. The article according to any one of claims 83-87, wherein the article is a product or a part of a product used in the electrical, household, packaging, automotive, toy or medical fields.
89. The article according to claim 88, wherein the article is a housing for household appliances, an automotive interior component, a children's toy, a household storage product, or a medical disposable syringe, or a part of these products.