A preparation method of a composite electrode and its application in nitrate-containing wastewater
By preparing La0.9FeO3-C composite electrode and activate it in electrochemical reaction, the problems of nitrate pollutant removal efficiency and cost in the prior art are solved, and the nitrate reduction effect is achieved with high efficiency, stable and low cost. It is suitable for use in the process of removing nitrate pollutants. Industrial application.
Patent Information
- Application Number
- CN202310220005.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When removing nitrate pollutants in water, the physical consumables are large and costly, and the biological stability is poor. Electrocatalytic reduction technology requires pretreatment of electrodes, which affects efficiency and cost.
La0.9FeO3-C composite electrode was prepared using La(NO3)3·6H2O, Fe(NO3)3·9H2O, citric acid and ethylene glycol. The carbon cloth substrate was treated by wet chemical oxidation method to form La0.9FeO3 -C composite electrode and activated in electrochemical reaction to achieve electrocatalytic reduction of nitrate.
It realizes efficient, stable and low-cost nitrate reduction to nitrogen, reduces environmental pollution, is suitable for natural water and sewage treatment, has green, gentle, environmentally friendly and simple characteristics, and is suitable for industrial production.
Smart Images

Figure CN116161752B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical water treatment, and in particular to a preparation method of a composite electrode and application of the composite electrode in nitrate-containing wastewater. Background Art
[0002] Nitrate is one of the main pollutants in water. At present, the common methods for removing nitrate from water are generally divided into physical methods, chemical methods and biological methods. The physical method is a method of removing nitrate from water through physical processes, including adsorption, distillation, ion exchange, reverse osmosis, electrodialysis, etc. Among them, modified adsorbent materials can improve the adsorption capacity, but a large amount of adsorbent materials are consumed; the ion exchange method also requires a large amount of regeneration agent, and the effluent needs to be treated before it can be discharged; the distillation method has high energy consumption and is only suitable for treating a small amount of water; reverse osmosis and electrodialysis have good nitrate removal effects, but the cost is high, and subsequent waste liquid is difficult to treat. In addition, physical methods can only adsorb or transfer nitrates, but cannot remove nitrate pollutants in chemical form. The biological process converts nitrates into nitrogen through microbial denitrification to remove nitrate pollution. It has stable effects, low costs, and the final product is nitrogen. It has little impact on the environment, but it also has disadvantages such as the operating environment and microbial growth are easily affected. As a new type of water pollution treatment technology, electrocatalytic reduction technology can realize the conversion of nitrates into nitrogen or lower valence ammonia nitrogen, and completely realize the removal of nitrates.
[0003] In recent years, electrocatalytic reduction technology has been widely used in the treatment of nitrate pollution due to its high efficiency and no secondary pollution. Nitrate reduction occurs on the cathode surface. The principle is that in an electrochemical reaction device, direct current is applied to the electrodes, and nitrate pollutants in the water body will undergo a reduction reaction on the catalytic layer on the cathode surface. Compared with biological denitrification and physical separation, electrocatalytic reduction technology relies on the electrolysis reaction on the electrode surface to directly reduce (pollutants directly obtain electrons and are reduced on the cathode) or indirectly reduce (reduced hydrogen is produced during the electrolysis process) pollutants, and has the advantages of high efficiency, low cost, and no need for external reducing agents.
[0004] The electrode material, electrolyte solution and the physical and chemical properties of wastewater are the three main factors that affect the efficiency of electrocatalytic reduction. The choice of electrode material directly affects the degradation efficiency of nitrate. On the one hand, there are large differences in the reduction performance of nitrate by different electrodes. On the other hand, the electrode also determines the current efficiency, stability and durability. The pretreatment of electrode materials is an indispensable key link, and this step lays a solid foundation for subsequent research. The electrode is activated by constant current electrochemical reduction method. Before the surface is electrically activated, the electrode has a large overpotential, resulting in slow response and increased energy consumption. After pretreatment, the electrode surface is activated, and the original electrode surface with higher stability and reproducibility is obtained. In order to achieve higher reduction rate and lower cost in the nitrate reduction process, metal oxides are used instead of precious metals. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a composite electrode and its application in nitrate-containing wastewater to solve the problems in the prior art.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing a composite electrode and its application in nitrate-containing wastewater, comprising the following steps:
[0007] Step 1: La(NO3)3·6H2O and Fe(NO3)3·9H2O are weighed, citric acid is used as a chelating agent, ethylene glycol is used as a polycondensation agent, mixed in pure water, and stirred evenly at room temperature to obtain a gel containing rare earth cations and metal cations;
[0008] Step 2: Drying the gel once to evaporate the water inside, so that the material is in a wet gel state; then drying the wet gel-like material twice to obtain a dry gel-like material;
[0009] Step 3: Grind the dry gel material and calcine it at high temperature to obtain a powdery material; grind it further and calcine it at high temperature for a second time, and cool it to obtain La 0.9 FeO3 powder;
[0010] Step 4: treating the hydrophilic conductive carbon cloth substrate by a wet chemical oxidation method, mixing a nitric acid solution with a sulfuric acid solution to obtain a mixed acid solution, and immersing the carbon cloth in the mixed acid solution;
[0011] Step 5: La 0.9 FeO3 powder, ethanol as solvent, and Nafion solution were mixed by ultrasonic for 1 hour to obtain a suspension, and the suspension was evenly dropped on the carbon cloth substrate and dried to obtain La 0.9 FeO3-C composite electrode.
[0012] Furthermore, in step 1, the molar concentration ratio of ethylene glycol, citric acid and metal ions in the solution is (7-8):(2-1):(0.95-1); and the metal ion concentration is 0.2-0.3 mol / L.
[0013] Further, in step 1, the metal ions include La Ⅲ and Fe Ⅲ , La Ⅲ and Fe Ⅲ The molar concentration ratio is (0.8~0.9):1.
[0014] Furthermore, in step 1, the molar concentration ratio of ethylene glycol, citric acid and metal ions in the solution is preferably 8:2:0.95; and the metal ion concentration is preferably 0.2375 mol / L.
[0015] Furthermore, in step 2, the primary drying temperature is 70-80° C., and the drying time is 10-12 h; preferably, the drying temperature is 80° C., and the drying time is 10 h.
[0016] Furthermore, in step 2, the secondary drying temperature is 100-120° C., and the drying time is 10-12 hours; preferably, the drying temperature is 120° C., and the drying time is 10 hours.
[0017] Furthermore, in step 3, the primary calcination condition is to increase the temperature at a rate of 5°C / min, the calcination temperature is 300-350°C, preferably 300°C, and the calcination time is 2-3h, preferably 2h; the secondary calcination condition is to increase the temperature at a rate of 5°C / min, the calcination temperature is 700-750°C, preferably 700°C, and the calcination time is 2-3h, preferably 2h.
[0018] Furthermore, in step 4, the mixed acid solution is a mixture of 10% nitric acid and 10% sulfuric acid in a volume ratio of 3:1; the soaking time is 20 to 24 hours, preferably 24 hours.
[0019] Furthermore, in step 5, the drying temperature is 70-80°C, preferably 80°C.
[0020] Furthermore, the La 0.9 The application method of FeO3-C composite electrode is: 0.9 The FeO3-C composite electrode was used as the cathode, the mesh ruthenium-iridium electrode was used as the anode, and a 50 mM sodium sulfate solution was used as the electrolyte. A constant current density of 15 mA / cm was continuously passed for 10 hours. 2 The composite electrode is activated by direct current. 0.9The FeO3-C composite electrode was used as the cathode, the mesh ruthenium-iridium electrode was used as the anode, and the 50mM sodium sulfate solution was used as the electrolyte. The distance between the anode and the cathode was controlled to be 0.5-1.5cm, and 15mA / cm 2 Direct current was used for electrocatalytic reduction of nitrate at a temperature of 20-30°C for 180 min.
[0021] Compared with the prior art, the present invention has the following beneficial effects: the present invention prepares La 0.9 The FeO3-C composite electrode can more effectively and rapidly electrocatalyze the reduction of nitrate to nitrogen, thus reducing the environmental pollution caused by nitrate. By treating the electrode surface with electric current, the nitrate catalytic active sites are changed, thereby obtaining an original electrode surface with high stability and good reproducibility, which is suitable for the removal of nitrate in natural water bodies and sewage without the need to adjust the pH. The present invention uses a series of electrochemical parameters to precisely control the catalyst surface microstructure, and has the characteristics of being green, mild, environmentally friendly, simple, low-cost, and easy to operate. In addition, the raw material source is wide, the production cost is low, and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0023] Figure 1 The present invention is La 0.9 Preparation flow chart of FeO3-C composite electrode;
[0024] Figure 2 is La prepared in Example 1 0.9 XRD patterns of FeO3-C composite electrode before and after electroactivation treatment;
[0025] Figure 3 It's La 0.9 Graph showing the effect of electrochemical reduction of nitrate at FeO3-C composite electrode. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The raw materials and their sources used in the present invention are as follows:
[0028] The carbon cloth substrate was purchased from Suzhou Shengernuo Technology Co., Ltd., model WOS1011; DuPont 5% Nafion solution was purchased from Suzhou Shengernuo Technology Co., Ltd., model D520; the mesh ruthenium-iridium electrode was purchased from Mingxuan Metal Materials, with a thickness of 1 mm, diamond holes, and a pore size of 1 mm×3 mm; La(NO3)3·6H2O (CAS No.: 10277-43-7), Fe(NO3)3·9H2O (CAS No.: 7782-61-8), citric acid (CAS No.: 77-92-9), ethylene glycol (CAS No.: 107-21-1), sodium sulfate (CAS No.: 7757-82-6), nitric acid (CAS No.: 7697-37-2), and sulfuric acid (CAS No.: 7757-82-6) were all purchased from Aladdin.
[0029] Example 1
[0030] (1)La 0.9 Preparation of FeO3 powder
[0031] Accurately weigh 2.4300g La(NO3)3·6H2O and 2.5191g Fe(NO3)3·9H2O solid powders and dissolve them in 25.0000mL deionized water to obtain a metal nitrate mixed solution, and stir it evenly at room temperature; at the same time, dissolve 5.2500g citric acid in 25.0000mL deionized water, stir it evenly, pour it into the above metal ion nitrate mixed solution, continue to stir it evenly, and then slowly add 5.6000mL of ethylene glycol. The metal ion concentration is 0.2375mol / L, of which the concentration of La(NO3)3·6H2O is 0.1125mol / L, the concentration of Fe(NO3)3·9H2O is 0.1250mol / L; the concentration of citric acid is 0.5000mol / L; the concentration of ethylene glycol is 2.0000mol / L. The mixed solution was placed in an oven at 80°C for 10 hours to dry all the water to obtain a wet gel; the wet gel was then dried at 120°C for 10 hours to obtain a dry gel; the obtained dry gel was ground with a mortar and calcined in a muffle furnace at 300°C for 2 hours, and the heating rate of the muffle furnace was 5°C / min; the obtained powdered material was cooled and further ground with a mortar, and then calcined in a muffle furnace at 700°C for 3 hours, and the heating rate of the muffle furnace was 5°C / min, and La was obtained after cooling. 0.9 FeO3 powder.
[0032] (2) Pretreatment of carbon substrate
[0033] The carbon cloth substrate needs to undergo a series of pretreatments, including cutting, wet chemical oxidation treatment, and ultrasonic water washing. The carbon cloth is cut into squares with a side length of 2 cm using tools such as scissors or blades; 10% nitric acid and 10% sulfuric acid are mixed in a volume ratio of 3:1, and the carbon cloth is immersed in the mixed solution for 24 hours, and ultrasonically treated under deionized water until the water is clear to ensure that there is no residual nitric acid and sulfuric acid.
[0034] (3)La 0.9 Preparation of FeO3-C composite electrode
[0035] Accurately weigh 0.0030 g of La prepared in step (1) 0.9 FeO3 powder, add 1.2000mL ethanol solution and 0.0060mL naphthol solution, mix the suspension by ultrasonic for 1 hour, use a pipette or dropper to evenly drop the suspension on the carbon cloth substrate prepared in step (2), and dry it at 80°C.
[0036] Example 2
[0037] Under normal temperature and pressure conditions, sodium sulfate and sodium nitrate are used as raw materials to simulate wastewater. 3.57mM sodium nitrate is used as the target pollutant, and 50mM sodium sulfate solution is used as the electrolyte solution to obtain simulated wastewater.
[0038] In the present invention, a dual-electrode system is used, including a cathode and an anode, and the distance between the anode and the cathode is 1.5 cm. 0.9 The FeO3-C composite electrode was used as the cathode, the 2 cm-long mesh ruthenium-iridium electrode was used as the anode, and the 50 mM sodium sulfate solution was used as the electrolyte. A constant current density of 15 mA / cm was continuously passed for 10 hours. 2 The composite electrode was activated by direct current. The activated electrode was placed in 50 mL of simulated wastewater to be treated and placed in a reactor. At room temperature and pressure, a current density of 15 mA / cm 2 Direct current is used for electrocatalytic reaction. After 180 minutes of reaction, the nitrate reduction rate in water can reach 85.6±0.6%.
[0039] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0040] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite electrode, characterized in that: The following steps are involved: Step 1: weigh La(NO3)3•6H2O and Fe(NO3)3•9H2O, use citric acid as a chelating agent and ethylene glycol as a polycondensation agent, mix them in pure water, and stir them evenly at room temperature to obtain a gel containing rare earth cations and metal cations; the molar concentration ratio of ethylene glycol, citric acid and metal ions in the solution is (7~8):(2~1):(0.95~1); the metal ion concentration is 0.2~0.3 mol / L; the metal ions include La(Ⅲ) and Fe(Ⅲ), and the molar concentration ratio of La(Ⅲ) and Fe(Ⅲ) is (0.8~0.9):1; Step 2: Drying the gel once to evaporate the water inside, so that the material is in a wet gel state; then drying the wet gel-like material twice to obtain a dry gel-like material; Step 3: Grind the dry gel material and calcine it once to obtain a powdery material; grind it and calcine it again, and cool it to obtain La 0.9 FeO3 powder; Step 4: treating the hydrophilic conductive carbon cloth substrate by a wet chemical oxidation method, mixing a nitric acid solution with a sulfuric acid solution to obtain a mixed acid solution, and immersing the carbon cloth in the mixed acid solution; Step 5: La 0.9 FeO3, ethanol as solvent, and Nafion solution were mixed by ultrasonic mixing to obtain a suspension, and the suspension was evenly dropped on the carbon cloth substrate and dried to obtain La 0.9 FeO3-C composite electrode.
2. The method for preparing a composite electrode according to claim 1, characterized in that: In step 2, the primary drying temperature is 70-80° C., and the drying time is 10-12 hours; the secondary drying temperature is 100-120° C., and the drying time is 10-12 hours.
3. The method for preparing a composite electrode according to claim 1, characterized in that: In step 3, the primary calcination condition is to increase the temperature at a rate of 5°C / min, the calcination temperature is 300-350°C, and the calcination time is 2-3h; the secondary calcination condition is to increase the temperature at a rate of 5°C / min, the calcination temperature is 700-750°C, and the calcination time is 2-3h.
4. The method for preparing a composite electrode according to claim 1, characterized in that: In step 4, the mixed acid solution is a mixture of nitric acid and sulfuric acid solution in a volume ratio of 3:1; the immersion time is 20 to 24 hours.
5. The method for preparing a composite electrode according to claim 1, characterized in that: In step 5, the drying temperature is 70-80°C.
6. A composite electrode prepared by the method for preparing a composite electrode according to any one of claims 1 to 5.
7. The use of a composite electrode according to claim 6, characterized in that: The composite electrode is activated and applied in nitrate-containing wastewater with La 0.9 The FeO3-C composite electrode is used as the cathode, the mesh ruthenium-iridium electrode is used as the anode, and the sodium sulfate solution is used as the electrolyte. Direct current is passed through to carry out the electrocatalytic reduction of nitrate.
8. The use of a composite electrode according to claim 7, characterized in that: The activation method of the composite electrode is: using sodium sulfate solution as electrolyte and La 0.9 The FeO3-C composite electrode is used as the cathode, and the mesh ruthenium-iridium electrode is used as the anode. Direct current is continuously passed through to activate the composite electrode.
9. The use of a composite electrode according to claim 7, characterized in that: The DC current density is 15 mA / cm 2 ; The electrocatalytic reduction temperature is 20~30℃, and the time is 180min; The distance between the anode and the cathode is 0.5~1.5cm.