A method for producing seamless pipes using a graded cooling process

Through the online cooling control and water quenching of the graded cooling process, the problems of high residual stress and cracking of the inner wall in the seamless pipe are solved, and the production of low-residual stress seamless pipes with low cost and simple processes is achieved, ensuring the high stiffness and straightness of the steel pipes Spend.

CN116162776BActive Publication Date: 2024-11-12BAOSHAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111410930.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-25
Publication Date
2024-11-12
Estimated Expiration
2041-11-25

AI Technical Summary

Technical Problem

The prior art reduces or eliminates residual stress in seamless pipes, which is costly and increases the production process, and it is difficult to effectively avoid the problem of cracking in the inner wall.

Method used

The graded cooling process is adopted, including online cooling and water quenching after rolling. By controlling the cooling speed and method of the steel pipe, the residual stress is reduced and the inner wall is avoided. The specific steps include water-cooling the outer wall and inner wall, controlling the cooling temperature and speed, and rotating cooling to Good uniformity, the inner wall cooling is delayed until the ferrite structure precipitates, ensuring mutual elimination of phase change and thermal stress.

Benefits of technology

The residual stress of the seamless pipe is significantly reduced, below 50MPa, avoiding additional annealing and physical stress removal methods, and the process flow is simple and easy to operate, ensuring the high stiffness and straightness of the steel pipe and avoiding cracking of the inner wall.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116162776B_ABST
    Figure CN116162776B_ABST
Patent Text Reader

Abstract

A method for producing seamless pipes by using a graded cooling process comprises the following steps: 1) smelting and casting, 2) soaking, 3) perforation, 4) continuous rolling, 5) reheating, 6) cooling, 7) straightening, 8) quenching, and 9) tempering. The present invention adopts a graded cooling process in the process of online controlled cooling and water quenching after rolling to increase the rigidity and straightness level of the steel pipe, effectively control the distribution of phase change and thermal stress over the entire wall thickness of the steel pipe, and control the precipitation of ferrite in the seamless pipe structure. When the inner wall of the prepared seamless pipe is free of cracks, no additional annealing and physical stress relief means are required, and a low residual stress seamless pipe can be obtained, and the process is simple and easy to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of seamless pipe preparation, in particular to a method for producing seamless pipes by adopting a graded cooling process. Background Art

[0002] Seamless pipes are widely used in oil and gas exploration, transportation, and engineering machinery. Residual stress has a great influence on their resistance to external pressure, internal pressure, and fatigue life. Currently, conventional means to reduce or eliminate residual stress include high-temperature stress relief annealing and mechanical physical methods, but such process methods are costly and increase the production process.

[0003] Chinese patent CN201810365440.5 discloses "a method for eliminating residual stress in quenched and tempered seamless steel pipes and the bidirectional chain cooling bed used therein", which eliminates residual stress by controlling the straightness of the steel pipe before quenching and tempering after rolling and the bidirectional chain of the cooling bed after quenching and tempering, thereby eliminating the quenching and tempering stress relief annealing process and achieving the purpose of cost reduction.

[0004] Chinese patent CN201420805596.8 discloses "asymmetric steel pipe straightening roller", which designs a special straightening roller to eliminate residual stress and oxide scale of the steel pipe by controlling the force on the steel pipe during the straightening process.

[0005] Chinese patent CN200910210718.2 discloses "a method for controlling the residual stress level of a conveying steel pipe". The patent derives a formula, and by measuring the elasticity of the steel pipe and comparing it with the formula, the residual stress level of the steel pipe is obtained. This is a method for measuring and characterizing the residual stress level. Summary of the invention

[0006] The object of the present invention is to provide a method for producing seamless pipes by adopting a graded cooling process. By adopting a graded cooling process during online controlled cooling and water quenching after rolling, cracking of the inner wall is avoided, and the residual stress of the obtained seamless pipe is significantly reduced. No additional annealing and physical stress relief means are required, and the process flow is simple and easy to operate; the residual stress of the obtained seamless pipe is less than 50MPa.

[0007] To achieve the above object, the technical solution of the present invention is:

[0008] A method for producing seamless pipes using a graded cooling process comprises the following steps:

[0009] 1) Smelting and casting;

[0010] 2) heating;

[0011] 3) Perforation;

[0012] 4) Continuous rolling;

[0013] 5) reheating;

[0014] 6) Cooling

[0015] After the steel pipe is stretched and reduced, only the outer wall of the steel pipe is water-cooled, and the cooling temperature of the steel pipe is controlled to be ≥Ar3, B f ≤The final cooling temperature of the steel pipe is ≤Bs-100℃, and the cooling rate is controlled at 25~35℃ / s;

[0016] 7) Straightening;

[0017] 8) Quenching

[0018] Ac3+30℃≤quenching temperature≤Ac3+60℃, then water cooling is used for graded cooling. The steel pipe rotates during the cooling process. When cooling, the outer wall of the steel pipe is first cooled by external water spraying. When the inner wall temperature is less than Ar3-70℃≤Ar3-30℃, water is injected into the steel pipe from one end until the cooling water fills the inner hole of the steel pipe and the steel pipe is cooled to room temperature;

[0019] 9) Tempering.

[0020] Preferably, in step 2), the heating temperature is 1250-1280° C. and the heating time is 3-4 hours.

[0021] Preferably, in step 3), the perforation temperature is 1100-1230°C.

[0022] Preferably, in step 4), the final rolling temperature is 800-1000°C.

[0023] Preferably, in step 5), the steel pipe is air-cooled to below Ar3-50°C and then heated to 950-980°C.

[0024] Preferably, in step 6), the tension reduction temperature is 850-900°C.

[0025] Preferably, in step 7), the steel pipe is straightened after being cooled to the final cooling temperature, and the steel pipe is naturally cooled to room temperature after straightening.

[0026] Preferably, the seamless pipe is made of conventional quenched and tempered alloy steel.

[0027] Preferably, the seamless pipe is made of low alloy steel with a Cr alloy content of ≤5wt.%, and the obtained seamless pipe microstructure is tempered troostite + ferrite, and the ferrite content in the structure from the outer wall to the inner wall of the seamless pipe is gradiently distributed, and the closer to the inner wall, the more ferrite content in the structure.

[0028] Preferably, the seamless pipe is made of a high alloy steel with a Cr alloy content of more than 5wt.%, and the obtained seamless pipe structure is a uniform tempered troostite structure.

[0029] The present invention adopts a graded cooling process during the online controlled cooling and water quenching process after rolling, which significantly reduces the residual stress of the seamless pipe. The present invention adopts water cooling after tension reduction, and only cools the outer wall, and controls the cooling start temperature ≥Ar3, B f ≤ Final cooling temperature ≤ B s -100℃, B f is the temperature at which the bainite phase transformation ends during cooling, B s It is the temperature at which the bainite phase transformation begins during the cooling process, and the cooling rate is controlled in the range of 25-35℃ / s during the cooling process. The main purpose of this process is to quickly cool and harden the steel pipe through homogenization cooling, ensuring the straightness of the steel pipe ≤2mm / m, while refining the rolled structure, laying the foundation for obtaining good performance matching after subsequent quenching and tempering. In addition, this cooling method reduces the residual stress level in the rolled state.

[0030] After the steel pipe is rapidly cooled to the final cooling temperature, it is immediately straightened. Warm straightening is beneficial to ensure straightness and reduce the residual stress level in the rolled state. After straightening, the straightness of the steel pipe is less than 1.5mm / m, and then it is placed on a cooling bed to cool naturally to room temperature.

[0031] The present invention adopts water cooling to perform graded cooling after quenching. The steel pipe is rotated during cooling. The outer wall of the steel pipe is first cooled by external water spraying. When Ar3-70℃≤inner wall temperature≤less than Ar3-30℃, the inner water spray is turned on to inject water into the steel pipe to cool the inner wall of the steel pipe. The cooling water fills the inner hole of the steel pipe and cools to room temperature.

[0032] The present invention adopts the principle of graded cooling process to cool the steel pipe:

[0033] 1. Since the external water spray cools the entire length of the steel pipe at the same time, the steel pipe rotates during cooling to achieve better cooling uniformity. When cooling the inner wall, the cooling water enters the steel pipe, and one end of the steel pipe is cooled first and the other end is cooled later, which increases the rigidity of the steel pipe. Its better cooling uniformity ensures a better straightness level of the steel pipe and avoids the larger residual stress caused by subsequent bending and straightening deformation of the pipe.

[0034] 2. The residual stress of the steel pipe is closely related to the phase change and thermal stress during the cooling process. The distribution of phase change and thermal stress over the entire wall thickness of the steel pipe can be effectively controlled through graded cooling, and the mutual cancellation of martensitic phase change stress and thermal stress can be achieved, which can effectively reduce the residual stress level of the steel pipe. In the technical solution described in the present invention, the graded cooling method of the outer wall first and then the inner wall is adopted. The phase change stress of the outer wall of the steel pipe is tensile stress, while the thermal stress is compressive stress. The phase change stress of the center of the steel pipe is compressive stress, while the thermal stress is tensile stress, and the two cancel each other out.

[0035] 3. The inner wall cooling transformation organization precipitates partial ferrite organization, rather than complete martensite organization, which can effectively reduce the residual stress of the inner wall. In the present invention, the inner wall phase change stress and thermal stress are both tensile stresses, but the inner wall is the late cooling surface. The inner wall cooling is not started until Ar3-70℃≤inner wall temperature≤less than Ar3-30℃. At this time, ferrite organization has been precipitated on the inner wall, which reduces the transformation ratio of martensite organization and reduces the phase change stress at the inner wall position, thereby effectively reducing the residual stress level within 1mm from the inner wall in the thickness direction of the cylinder tube and avoiding cracking of the inner wall.

[0036] Beneficial effects of the present invention:

[0037] The present invention adopts different graded cooling processes in the process of online controlled cooling and water quenching after rolling, that is, after the steel pipe is stretched and quenched. On the one hand, the rigidity and straightness level of the steel pipe are increased, thereby avoiding the large residual stress caused by subsequent bending and straightening deformation of the pipe; on the other hand, the distribution of phase transformation and thermal stress over the entire wall thickness of the seamless pipe is controlled to achieve mutual cancellation of martensitic phase transformation stress and thermal stress, thereby effectively reducing the residual stress level of the steel pipe; finally, by controlling the precipitation of ferrite structure in the microstructure of the seamless pipe, the residual stress level of the inner wall is effectively reduced, thereby avoiding the occurrence of cracking of the inner wall.

[0038] The seamless pipe prepared by the method of the present invention can obtain low residual stress without additional annealing and physical stress relief means, and the process is simple and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a picture of the residual stress measurement of seamless pipes prepared by traditional technology using the slit method.

[0040] Figure 2 This is a picture of the residual stress of the seamless pipe of Example 1 of the present invention measured by the slit method. DETAILED DESCRIPTION

[0041] The present invention will be further described below by way of examples.

[0042] The specific process parameters of the embodiments of the present invention are shown in Table 1, the properties of the seamless pipes obtained in the embodiments and comparative examples are shown in Table 2, and the residual stress is measured with reference to the ISO / TR 10400 standard.

[0043] Figure 1 and Figure 2 The pictures are respectively of the seamless pipe prepared by the conventional process and the seamless pipe prepared by Example 1 of the present invention measured by the slit method for residual stress.

[0044] Depend on Figure 1 , Figure 2It can be seen that the gap of the seamless pipe obtained by the method of the present invention is smaller than that of the seamless pipe prepared by the traditional process. Obviously, the residual stress of the seamless pipe obtained by the method of the present invention is significantly smaller than that of the seamless pipe prepared by the traditional process.

[0045] It can be seen from Table 3 that the inner wall of the seamless pipe obtained by the present invention has no cracks, and the residual stress is lower than 50 MPa, and the residual stress can even be 0. In addition, the comparative example processes other than the embodiments of the present invention cannot meet the requirements of the present invention, and the residual stress of the obtained seamless pipe is high, and the inner wall may also crack.

[0046]

[0047]

Claims

1. A method for producing seamless pipes using a graded cooling process, characterized in that: The following steps are involved: 1) Smelting and casting; 2) heating; 3) Perforation; 4) Continuous rolling; 5) reheating; 6) Cooling After the steel pipe is stretched and reduced, only the outer wall of the steel pipe is water-cooled, and the cooling temperature of the steel pipe is controlled to be ≥Ar3, B f ≤Steel pipe final cooling temperature≤B s -100℃, cooling rate controlled at 25~35℃ / s; 7) Straightening; 8) Quenching Ac3+30℃≤quenching temperature≤Ac3+60℃, then water cooling is used for graded cooling. The steel pipe rotates during the cooling process. When cooling, the outer wall of the steel pipe is first cooled by external water spraying. When Ar3-70℃≤inner wall temperature≤Ar3-30℃, water is injected into the steel pipe from one end until the cooling water fills the inner hole of the steel pipe until the steel pipe is cooled to room temperature; 9) Tempering.

2. The method for producing seamless pipes using a graded cooling process according to claim 1, characterized in that: In step 2), the heating temperature is 1250-1280° C. and the heating time is 3-4 hours.

3. The method for producing seamless pipes by using a graded cooling process according to claim 1, characterized in that: In step 3), the perforation temperature is 1100-1230°C.

4. The method for producing seamless pipes by using a graded cooling process according to claim 1, characterized in that: In step 4), the final rolling temperature is 800-1000°C.

5. The method for producing seamless pipes by using a graded cooling process according to claim 1, characterized in that: In step 5), the mixture is first cooled by air to below Ar3-50°C and then heated to 950-980°C.

6. The method for producing seamless pipes by using a graded cooling process according to claim 1, characterized in that: In step 6), the tension reduction temperature is 850-900°C.

7. The method for producing seamless pipes by using a graded cooling process as claimed in claim 1, characterized in that: In step 7), the steel pipe is straightened after being cooled to the final cooling temperature, and the steel pipe is naturally cooled to room temperature after straightening.

8. The method for producing seamless pipes by using a graded cooling process as claimed in claim 1, characterized in that: The seamless pipe is made of conventional quenched and tempered alloy steel.

9. The method for producing seamless pipes by using a graded cooling process as claimed in claim 8, characterized in that: The seamless pipe is made of low alloy steel with a Cr alloy content of ≤5wt.%, and the obtained seamless pipe microstructure is tempered troostite+ferrite, and the ferrite content in the seamless pipe structure from the outer wall to the inner wall is distributed in a gradient, and the closer to the inner wall, the more ferrite content in the structure.

10. The method for producing seamless pipes by using a graded cooling process according to claim 8, characterized in that: The seamless pipe is made of high alloy steel with a Cr alloy content greater than 5wt.%, and the obtained seamless pipe structure is a uniform tempered troostite structure.