A preparation method and application of porous carbon material
The ZIF-67/carbon material composite product is generated by a hydrothermal method and annealed to form a porous carbon material, which solves the problem of poor contact between active materials and base materials in flexible batteries and achieves the preparation of porous carbon materials with high electrochemical performance, which is suitable for Supercapacitors and flexible batteries.
Patent Information
- Application Number
- CN202211722254.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-30
AI Technical Summary
It is difficult to prepare porous carbon materials with high electrochemical properties using existing technology, especially in flexible batteries where poor contact between active materials and flexible base materials affects battery performance.
By dissolving cobalt salt and organic ligands in a solvent for a hydrothermal reaction, a ZIF-67/carbon material composite product is generated, and annealed under an inert gas atmosphere to form a porous carbon material, which simplifies the process and improves the material's properties. Specific capacitance and rate performance.
The porous carbon material has achieved high specific capacitance, excellent rate performance, energy density and power density. It is suitable for cathode materials of flexible batteries and supercapacitors, and the process is simple and easy for industrial production.
Smart Images

Figure CN116199205B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of energy storage materials, and specifically relates to a preparation method and application of a porous carbon material. Background Art
[0002] In recent years, with the massive consumption of fossil energy and the worsening of environmental pollution, the development of new energy and devices has attracted much attention. Among many new energy materials, carbon materials are widely used in supercapacitors due to their excellent conductivity. Carbon materials mainly include porous carbon, graphene, carbon nanotubes, carbon fibers, etc. Among them, the precursors of porous carbon are widely available and low in cost. Various natural biomass materials can also be used as precursors of porous carbon.
[0003] For example, carbon cloth, as one of the carbon materials, can also be used as a base material for porous carbon materials.
[0004] Porous carbon materials with carbon cloth as the substrate have excellent electrical conductivity, physical and chemical stability, and also maintain good electrochemical properties and gas permeability. These advantages make porous materials made of carbon cloth widely used in many fields. Through research, it is found that carbon cloth can be used as a substrate for flexible batteries. Due to its excellent structural stability, high conductivity and commercial availability, unlike traditional batteries, flexible electrodes usually do not contain adhesives and conductive additives, and the electrochemical properties of carbon cloth are still stable under the deformation of the pole piece. Therefore, carbon cloth is a substrate that is very suitable for flexible devices. In order to develop high-performance flexible batteries, good contact between the active material and the flexible substrate material is urgently needed.
[0005] Therefore, how to prepare porous carbon materials with high electrochemical performance is of great practical application value. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing a porous carbon material.
[0007] The invention also provides a porous carbon material.
[0008] According to one aspect of the present invention, a method for preparing a porous carbon material is provided, comprising the following steps:
[0009] The cobalt salt and the organic ligand are dissolved in a solvent, and the carbon material is added thereto for a hydrothermal reaction to obtain a ZIF-67 / carbon material composite product;
[0010] The ZIF-67 / carbon material composite product is annealed to obtain a porous carbon material.
[0011] In some embodiments of the present invention, the cobalt salt includes at least one of cobalt nitrate, cobalt acetate, cobalt carbonate, cobalt sulfate and hydrates thereof.
[0012] In some preferred embodiments of the present invention, the hydrate thereof may include at least one of cobalt nitrate hexahydrate, cobalt acetate tetrahydrate, cobalt carbonate hexahydrate and cobalt sulfate heptahydrate.
[0013] In some embodiments of the present invention, the organic ligand includes at least one of trimesic acid, terephthalic acid, and 2-nitroimidazole.
[0014] Preferably, the organic ligand is 2-methylimidazole.
[0015] In some embodiments of the present invention, the carbon material includes at least one of carbon paper, foamed graphite, bamboo charcoal and charcoal.
[0016] Preferably, the carbon material is carbon cloth.
[0017] In some embodiments of the present invention, the molar ratio of the cobalt salt to the organic ligand is 1:50-150; preferably, the molar ratio of the cobalt salt to the organic ligand is 1:70-130; preferably, the molar ratio of the cobalt salt to the organic ligand is 1:80-120.
[0018] In some embodiments of the present invention, the volume ratio of the molar number of the cobalt salt to the solvent is 0.2-1.0 mol:10 mL; preferably, the volume ratio of the molar number of the cobalt salt to the solvent is 0.2-0.7 mmol:10 mL; more preferably, the volume ratio of the molar number of the cobalt salt to the solvent is 0.2-0.5 mmol:10 mL.
[0019] In some embodiments of the present invention, the solvent is a mixture of water and an organic solvent.
[0020] In some preferred embodiments of the present invention, the volume ratio of water to the organic solvent is 1:1-4; preferably, the volume ratio of water to the organic solvent is 1:1-3.
[0021] In some embodiments of the present invention, the organic solvent includes at least one of N,N-dimethylformamide, nitrogen methyl pyrrolidone, ethanol, butanol, acetone, cyclohexane, cyclohexanone and methyl butyl ketone.
[0022] In some preferred embodiments of the present invention, the organic solvent is N,N-dimethylformamide.
[0023] In some embodiments of the present invention, the hydrothermal reaction temperature is 110-130°C, preferably 115-125°C, for example, about 115°C, about 120°C or about 125°C.
[0024] In some embodiments of the present invention, the time is 1 to 2 hours.
[0025] In some preferred embodiments of the present invention, the hydrothermal reaction temperature is about 120° C. and the time is about 2 h.
[0026] In some preferred embodiments of the present invention, a drying step is further included after the hydrothermal reaction; preferably, the drying temperature is 60-100° C. and the drying time is 6-12 hours.
[0027] In some embodiments of the present invention, annealing is performed in a protective gas to promote carbonization of the intermediate product. The protective gas is at least one of nitrogen or an inert gas. Preferably, the inert gas is argon and / or helium. More preferably, the protective gas is nitrogen.
[0028] In some embodiments of the present invention, the annealing temperature is 700-1000° C., for example, the heating rate is 1-10° C. / min, and the holding time is 1-4 hours. The temperature may be naturally lowered after annealing.
[0029] The present invention utilizes a hydrothermal method to grow ZIF on a carbon material, which takes a short time and has a fast reaction. The ZIF particles are carbonized by calcining at an excessively high temperature in an inert gas atmosphere, leaving only elemental cobalt, and a porous carbon material is formed by etching. Furthermore, the elemental cobalt can also be removed by further acid corrosion, and the performance will not change significantly.
[0030] According to another aspect of the present invention, a porous carbon material is provided, which is prepared by the above-mentioned preparation method.
[0031] The present invention also particularly proposes a porous carbon cloth material. The porous carbon cloth material has a porous structure, an increased surface area, and a small impedance, and can have electrochemical properties such as higher specific capacitance, excellent rate performance, energy density, and power density.
[0032] According to yet another aspect of the present invention, a positive electrode material is provided, which comprises the porous carbon material mentioned above.
[0033] According to another aspect of the present invention, an aqueous zinc hybrid supercapacitor is provided, which includes the above-mentioned positive electrode material.
[0034] According to some embodiments of the present invention, an aqueous zinc hybrid supercapacitor comprises a positive electrode, a separator, an electrolyte and a negative electrode. Specifically, the positive electrode comprises the above-mentioned positive electrode material; the separator is selected from glass fiber; the electrolyte comprises a soluble zinc salt; and the negative electrode is a zinc sheet.
[0035] The present invention uses carbon material as a growth substrate, homogeneously nucleates by a hydrothermal method, grows high-density ZIF-67 on the growth substrate, and generates a porous carbon material by high-temperature carbonization. The method is simple and easy to operate and is suitable for industrial production. Due to the porous structure of the prepared porous carbon material, it has higher specific capacitance, excellent rate performance, energy density, power density and other electrochemical properties when used as an electrode material for a supercapacitor. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 a is a SEM image of ZIF-67 / carbon cloth prepared in Example 1; Figure 1 b is a SEM image of the porous carbon cloth material prepared in Example 2;
[0037] Figure 2 is the electrochemical performance diagram of the porous carbon cloth material prepared in Example 2 and the blank carbon cloth, wherein Figure 2 a is the AC impedance diagram; Figure 2 b is 1 mA cm -1 The constant current charge and discharge curve diagram below.
[0038] Figure 3 The carbon cloth materials prepared in Comparative Example 1 and Comparative Example 2 were subjected to 1 mA cm -1 The constant current charge and discharge curve diagram below. DETAILED DESCRIPTION
[0039] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0040] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0041] Example 1
[0042] This embodiment provides a ZIF-67 / carbon cloth composite material.
[0043] 0.08 g of cobalt nitrate hexahydrate and 0.8 g of 2-methylimidazole were dissolved in a mixed solution of 10 mL of N,N-dimethylformamide and 5 mL of deionized water. After sufficient stirring, the mixture was transferred into a 25 mL polytetrafluoroethylene liner and placed in a reactor. The reactor was subjected to hydrothermal reaction at 120 °C in an oven for 2 h.
[0044] After the reaction is completed, the product is taken out and dried to obtain the ZIF-67 / carbon cloth composite material.
[0045] Example 2
[0046] This embodiment provides a porous carbon cloth material. The raw materials and preparation method are the same as those in Example 1. The obtained ZIF-67 / carbon cloth composite material is placed in a tubular furnace, heated to 900°C at a heating rate of 5°C / min under an inert gas atmosphere, kept at 900°C for 1 hour, and finally cooled naturally.
[0047] After the reaction is completed, a porous carbon cloth material is obtained.
[0048] Comparative Example 1
[0049] This embodiment provides a carbon cloth material. The raw materials and preparation method are the same as those in Embodiment 2, except that the hydrothermal temperature is changed to 100°C.
[0050] Comparative Example 2
[0051] This comparative example provides a carbon cloth material. The raw materials and preparation method are the same as those in Example 2, except that the hydrothermal temperature is changed to 140°C.
[0052] Performance Testing
[0053] The porous carbon cloth material prepared in the above implementation was used as the positive electrode material of the zinc ion hybrid supercapacitor and used to test the electrochemical performance. The following electrochemical performance tests were all carried out in an electrolytic cup environment, and the electrolyte was 2M ZnSO 4 aqueous solution, the positive electrode is the prepared porous carbon cloth material, the negative electrode is a zinc sheet, and the electrochemical workstation is CHI660E.
[0054] Figure 1 a and Figure 1 b are SEM images of ZIF-67 / carbon cloth prepared in Example 1 and porous carbon cloth prepared in Example 2. It can be seen from the figure that in Example 1, highly densely arranged ZIF-67 particles grow on the carbon cloth substrate; while in Example 2, the carbon cloth has many more holes than the smooth surface.
[0055] from Figure 2 It can be seen from a that the impedance of the porous carbon cloth material prepared in Example 2 is significantly lower than that of the blank carbon cloth, and Figure 2 In b, the constant current charge and discharge curve of the porous carbon cloth material prepared in Example 2 is significantly better than that of the blank carbon cloth.
[0056] Figure 3 The carbon cloth materials prepared in Comparative Example 1 and Comparative Example 2 show the -1The constant current charge-discharge curve diagram under . Among them, in comparative example 1, due to the growth of too little ZIF-67, the carbon cloth cannot form a porous structure and the performance is poor. In comparative example 2, the performance of the prepared carbon cloth material is poor, possibly due to the excessive residual cobalt element.
[0057] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a porous carbon cloth material, characterized in that: The following steps are involved: The cobalt salt and the organic ligand are dissolved in a solvent, and carbon cloth is added thereto for a hydrothermal reaction to obtain a ZIF-67 / carbon cloth composite product; Annealing the ZIF-67 / carbon cloth composite product to obtain the porous carbon cloth; the solvent is a mixture of water and an organic solvent; The hydrothermal reaction temperature is 110-130°C and the reaction time is 1-2h; The annealing temperature is 900°C or 1000°C; the holding time is 1-4 h; The annealing is performed in a protective gas; the protective gas is at least one of nitrogen or an inert gas.
2. The preparation method according to claim 1, characterized in that: The cobalt salt comprises at least one of cobalt nitrate, cobalt acetate, cobalt sulfate and hydrates thereof; and the organic ligand is 2-methylimidazole.
3. The preparation method according to claim 1, characterized in that The molar ratio of the cobalt salt to the organic ligand is 1:50-150; the volume ratio of the molar number of the cobalt salt to the solvent is 0.2-0.7 mmol:10 mL.
4. The preparation method according to claim 1, characterized in that: The solvent is a mixture of water and an organic solvent; the volume ratio of water to the organic solvent is 1:1-4; the organic solvent includes at least one of N,N-dimethylformamide, nitrogen methyl pyrrolidone, ethanol, butanol, acetone, cyclohexane, cyclohexanone and methyl butanone.
5. The preparation method according to claim 1, characterized in that: The protective gas is at least one of argon, nitrogen and helium.
6. The preparation method according to any one of claims 1 to 5, characterized in that The heating rate of the annealing is 1-10°C / min.
7. A porous carbon cloth, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 6.
8. A positive electrode material, characterized in that It comprises the porous carbon cloth as claimed in claim 7.
9. An aqueous zinc hybrid supercapacitor, characterized in that: It comprises the positive electrode material according to claim 8.