A CrW alloy target material and preparation method thereof
By optimizing the powder particle size and molding process, a high-density CrW alloy target was prepared, which solved the problems of material brittleness and difficulty in processing, and achieved the improvement of W element ratio and wide application.
Patent Information
- Application Number
- CN202211734636.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The existing CrW target preparation process has problems such as brittle and hard materials, difficult processing, high cost and insufficient W element ratio, which limits its wide application.
By optimizing the powder particle size and molding process, using a three-dimensional mixer to mix Cr powder and W powder, perform degassing treatment, thermal isostatic molding, electroplating treatment and diffusion welding, a CrW alloy with a maximum atomic ratio of 50% of W elements was prepared. Target material.
It achieves high density and good diffusion welding effect of CrW alloy targets, solves the problems of material brittleness and hardness and processing difficulty, and expands its application range.
Smart Images

Figure CN116200639B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hard coatings, and in particular relates to a CrW alloy target material and a preparation method thereof. Background Art
[0002] The application field of CrW targets is becoming more and more extensive. There are two main target preparation processes. One is to prepare by hot pressing and sintering. Chromium and tungsten undergo alloying reaction under high temperature and high pressure for a long time. The obtained target material is hard and brittle, which is not conducive to subsequent machining. The other is to obtain pre-alloyed powder by high-energy ball milling, and then obtain the target material by degassing hot isostatic pressing. This process is cumbersome, the cost of high-energy ball milling is high, and it is not conducive to industrial production.
[0003] In addition, as the proportion of W element in CrW target increases, the material becomes harder and more brittle, the shape of the processed product is limited, and the difficulty and cost of machining are greatly increased. At present, the proportion of W element in CrW target prepared by hot pressing and high-energy ball milling process is generally less than 20% atomic ratio, such as the chromium-tungsten alloy target obtained by the invention patent with authorization number CN105345007B, in which the atomic percentage of chromium is 80-99% and tungsten is 1-20%. However, CrW target with 20% atomic ratio of W element can no longer meet the needs of wide application. Summary of the invention
[0004] In order to solve the above problems, the present invention aims to provide a CrW alloy target and a preparation method thereof. The present invention prepares a CrW alloy target with a W atomic ratio of up to 50% by optimizing the powder particle size and the molding process.
[0005] To achieve the above object, the present invention provides a method for preparing a CrW alloy target, which specifically comprises the following steps:
[0006] S1. Mixing Cr powder and W powder in a predetermined ratio, wherein the atomic ratio of W element in the predetermined ratio is 5 to 50%, and the particle size of Cr powder is less than 30 μm;
[0007] S2. The mixed powder is loaded into the encapsulation mold for degassing;
[0008] S3. The degassed package is subjected to hot isostatic pressing;
[0009] S4. The hot isostatic pressing process is followed by removing the jacket from the blank, and then cutting it into target pieces of corresponding sizes, and grinding both end surfaces of the target piece;
[0010] S5. Sandblasting the two end surfaces of the target after grinding;
[0011] S6. Electroplating the two end surfaces of the target after sandblasting;
[0012] S7. The electroplated target sheet is stacked with an alloy backing plate of the same size and loaded into a sleeve mold for degassing;
[0013] S8. The degassed package is subjected to diffusion welding;
[0014] S9. Remove the sheath from the target sheet after diffusion welding, and then process it into a target material of a desired shape, thereby obtaining a CrW alloy target material with a backing plate.
[0015] The present invention adopts the above technical scheme, and adopts a simple three-dimensional mixer to mix materials during mixing. The process is simple and easy to operate, and the use of complex high-energy ball milling equipment is avoided, which makes the mixing process more complicated and the cost relatively high; and the Cr powder particle size is controlled to be less than 30μm during mixing, so that when Cr powder and W powder are mixed, the smaller the Cr powder particle size is, and the closer the Cr powder particle size is to the W powder particle size, the more uniform the W element is dispersed in the Cr matrix, and the high content of W is avoided. It is not easy to disperse evenly and the local agglomeration is not easy to be dense in the Cr matrix, and finally the W atomic ratio can be as high as 50%, and the target material density is good. By electroplating the two end faces of the target material, that is, the front and back sides of the target material, the workers do not need to distinguish between the two sides during operation, and can place any side to prevent mistakes. Finally, by welding a layer of easy-to-machine material at the bottom of the target material, the problem that the target material is brittle and hard and is not easy to be processed into a complex shape target material is solved, so that the target material is more widely used. Combining hot isostatic pressing with diffusion welding to connect the back plate and the target material reduces the processing difficulty and enables the combination to be realized compared with the hot isostatic pressing of the back plate directly with the target material powder. Because it is difficult to combine the target material powder and the back plate directly by hot isostatic pressing, the powder is packed in the package and becomes a dense target material through hot isostatic pressing. The shrinkage is very large, and it can even reach up to 40% depending on the different powder particle size composition. The back plate is a dense material and will not shrink during the hot isostatic pressing process. In addition, the hot isostatic pressing processes of the two are also different. The temperature required for diffusion welding cannot be too high and must be lower than the melting point of the back plate (such as Cu). The temperature of the first hot isostatic pressing of CrW reaches 1300℃, which is far higher than the melting point of the copper back plate, so it cannot be achieved by hot isostatic pressing in one time.
[0016] Furthermore, in step S1, the particle size of the W powder is 10-30 μm.
[0017] Furthermore, in step S1, the atomic ratio of the W element in the predetermined ratio is 20-50%.
[0018] Further, in step S2, the degassing and heat preservation temperature during the degassing treatment is 350-500°C (such as 350°C, 400°C, 450°C, 500°C).
[0019] Furthermore, in step S2, the degassing vacuum degree during the degassing treatment is 1*10 -3 ~9*10 -3 Pa (such as 1*10 -3 Pa, 2*10 -3 Pa, 3*10 -3 Pa, 4*10 -3 Pa, 5*10 -3 Pa, 6*10 -3 Pa, 7*10 -3 Pa, 8*10 -3 Pa, 9*10 -3 Pa).
[0020] Further, in step S3, the processing temperature during the hot isostatic pressing process is 1200°C to 1400°C (such as 1200°C, 1250°C, 1300°C, 1350°C, 1400°C), preferably 1300°C.
[0021] Further, in step S3, the pressure during the hot isostatic pressing process is 100-150 MPa (such as 100 MPa, 110 MPa, 120 MPa, 130 MPa, 140 MPa, 150 MPa), preferably 130 MPa.
[0022] Furthermore, in step S3, the heat preservation and pressure holding time during the hot isostatic pressing process is 1 to 4 hours (such as 1 hour, 2 hours, 3 hours, 4 hours).
[0023] Furthermore, in step S4, the cutting is performed using a medium-speed wire cutting machine.
[0024] Furthermore, in step S4, after the grinding process, the flatness of the two end surfaces of the target piece is less than 0.05 mm (such as 0.01 mm, 0.02 mm, 0.03 mm, 0.04 mm). Through the grinding process, the wire cutting marks are smoothed to ensure that the two end surfaces of the target piece are flat.
[0025] Further, in step S5, after the sandblasting, the roughness of the two end surfaces of the target sheet is not less than Ra3.6 (such as Ra3.6, Ra3.7, Ra3.8, Ra3.9, Ra4.0). The roughness is increased by sandblasting, thereby improving the welding bonding strength, because the surface is smooth after the plane is ground, the roughness is low, and the bonding strength of the coating is poor, so sandblasting is used for roughening.
[0026] Further, in step S6, the electroplating treatment is a nickel layer electroplating treatment, and the coating thickness is about 0.1-0.3 mm (such as 0.1 mm, 0.15 mm, 0.2 mm, 0.25 mm, 0.3 mm). The electroplated nickel layer has high chemical stability, and has a strong bonding force with the CrW target substrate. The nickel plating layer and the copper back plate are infinitely solid-dissolved and diffused with each other, and it is easy to form a good welding interface. At the same time, the thermal expansion coefficient of nickel is between the two welding materials, which can effectively reduce the welding stress, thereby making the welding interface better and the welding rate higher.
[0027] Furthermore, in step S7, the alloy back plate can be made of Cu, Mo and their alloys. Cu has good thermal and electrical conductivity and is a preferred back plate material for the target material; Mo has a small thermal expansion coefficient and relatively higher strength and is also a preferred back plate material; Cu and Mo can be made into alloys, and by adjusting their ratio, a material with good comprehensive performance can be designed and produced as a back plate.
[0028] Further, in step S7, the degassing and heat preservation temperature during the degassing treatment is 300-400°C (such as 300°C, 350°C, 400°C).
[0029] Furthermore, in step S7, the degassing vacuum degree during the degassing treatment is not greater than 2*10 -2 Pa (such as 2*10 - 2 Pa, 1*10 -2 Pa, 9*10 -3 Pa, 8*10 -3 Pa, 7*10 -3 Pa, 6*10 -3 Pa, 5*10 -3 Pa).
[0030] Further, in step S8, the treatment temperature during the diffusion welding treatment is 500°C-950°C (such as 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C), preferably 750°C.
[0031] Further, in step S8, the pressure during the diffusion welding process is 100-150 MPa (such as 100 MPa, 110 MPa, 120 MPa, 130 MPa, 140 MPa, 150 MPa).
[0032] Furthermore, in step S8, the heat preservation time during the diffusion welding process is 3-6 hours (such as 3 hours, 4 hours, 5 hours, 6 hours).
[0033] Further, in step S8, the diffusion welding process is performed by a hot isostatic press.
[0034] Further, in step S9, the processing is machining, specifically, processing by a slicer.
[0035] A CrW alloy target material prepared by the above preparation method comprises Cr and W in a predetermined ratio, wherein the atomic ratio of the W element is 5-50%.
[0036] Furthermore, the relative density of the CrW alloy target is ≥99%.
[0037] The CrW alloy target material of the present invention has uniform structure, no segregation, no agglomeration, etc., and a density of more than 99%.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The present invention prepares a CrW alloy target material with an atomic ratio of W element reaching 50% and a density of more than 99% through the HIP process, and achieves a good diffusion welding effect between the back plate and the target piece through surface modification nickel plating and HIP diffusion welding, thereby solving the problem of difficult machining. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is a schematic diagram of the preparation method of the present invention;
[0041] Figure 2 Cr obtained in Example 1 95 Microstructure of W5 alloy;
[0042] Figure 3 Cr obtained in Example 2 92 Microscopic morphology of W8 alloy;
[0043] Figure 4 Cr obtained in Example 3 90 W 10 Alloy micromorphology;
[0044] Figure 5 Cr obtained in Example 4 70 W 30 Alloy micromorphology;
[0045] Figure 6 Cr obtained in Example 5 50 W 50 Alloy micromorphology;
[0046] Figure 7 Cr obtained in Example 6 90 W 10 Alloy micromorphology;
[0047] Figure 8Cr obtained in Example 7 90 W 10 Alloy micromorphology;
[0048] Fig. 9 Cr obtained in Comparative Example 1 95 Microstructure of W5 alloy;
[0049] Fig.10 Cr obtained in Comparative Example 2 70 W 30 Alloy micromorphology;
[0050] Fig.11 Cr obtained in Comparative Example 3 70 W 30 Alloy micromorphology;
[0051] Fig.12 Cr obtained in Comparative Example 4 70 W 30 Microstructure of alloy. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0053] The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0054] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0055] In the present invention, unless otherwise specified and / or described, all numerical values involving the amounts of components are "parts by weight" from beginning to end. The process parameters in the following examples without specifying specific conditions are usually based on conventional conditions.
[0056] Examples 1-5
[0057] A method for preparing a CrW alloy target, the process is as follows Figure 1 As shown, the specific steps include:
[0058] S1. Mixing Cr powder and W powder in a predetermined ratio, wherein the atomic ratio of W element in the predetermined ratio is 5 to 50%, the particle size of Cr powder is 25 μm, and the particle size of W powder is 10 μm;
[0059] S2. The mixed powder is placed in a package mold for degassing. The degassing temperature is 400°C and the degassing vacuum is 4*10 -3 Pa;
[0060] S3. The degassed package is placed in a hot isostatic pressing furnace for hot isostatic pressing at a temperature of 1300°C, a pressure of 130MPa, and a holding time of 1h;
[0061] S4. The hot isostatic pressing process is followed by removing the jacket from the blank, and then cutting it into target pieces of corresponding sizes using a medium wire cutting machine, and grinding both end surfaces of the target piece to a flatness of less than 0.05 mm;
[0062] S5. The two end surfaces of the target piece after grinding are sandblasted so that the roughness of the two end surfaces of the target piece is not less than Ra3.6;
[0063] S6. Electroplating the two end surfaces of the target after sandblasting, specifically electroplating nickel layer, the coating thickness is about 0.01-0.1mm;
[0064] S7. Stack the electroplated target and the alloy backing plate of the same size together and put them into the encapsulation mold for degassing. The alloy backing plate is made of Cu, the degassing temperature is 300-400℃, and the degassing vacuum is 2*10 -2 Pa;
[0065] S8. The degassed package is placed in a hot isostatic press for diffusion welding at a temperature of 900°C, a pressure of 100-150MPa, and a holding time of 4h;
[0066] S9. The target piece after diffusion welding is removed from the jacket, and then processed into a target material of a desired shape by a slicer, to obtain a CrW alloy target material with a backing plate;
[0067] The specific preparation process parameters of Examples 1-5 and the components of the obtained CrW alloy target are recorded in Table 1. The microstructures of the obtained alloys are shown in Figure 2-6 middle.
[0068] Example 6
[0069] A method for preparing a CrW alloy target, which differs from Example 3 in that: S8. The package after degassing is placed in a hot isostatic press for diffusion welding, with a treatment temperature of 600° C., a pressure of 135 MPa, and a holding time of 4 h;
[0070] The rest of the settings are the same as those in Example 3.
[0071] The specific preparation process parameters and the composition of the obtained CrW alloy target are recorded in Table 1. The microstructure morphology of the obtained alloy is shown in Figure 7 middle.
[0072] Example 7
[0073] A method for preparing a CrW alloy target, which differs from Example 3 in that: S8. The package after degassing is placed in a hot isostatic press for diffusion welding, with a treatment temperature of 800° C., a pressure of 135 MPa, and a holding time of 4 h;
[0074] The rest of the settings are the same as those in Example 3.
[0075] The specific preparation process parameters and the composition of the obtained CrW alloy target are recorded in Table 1. The microstructure morphology of the obtained alloy is shown in Figure 8 middle.
[0076] Comparative Example 1
[0077] A method for preparing a CrW alloy target, which differs from Example 1 in that, step S1. Cr powder and W powder are uniformly mixed in a predetermined ratio, wherein the atomic ratio of W element in the predetermined ratio is 5%, the particle size of Cr powder is 150 μm, and the particle size of W powder is 10 μm;
[0078] The rest of the settings are the same as those in Example 1.
[0079] The specific preparation process parameters and the composition of the obtained CrW alloy target material of Comparative Example 1 are recorded in Table 1. The microstructure morphology of the obtained alloy is shown in Fig. 9 middle.
[0080] Comparative Example 2
[0081] A method for preparing a CrW alloy target, which differs from Example 4 in that, step S1. Cr powder and W powder are mixed uniformly in a predetermined ratio, wherein the atomic ratio of W element in the predetermined ratio is 30%, the particle size of Cr powder is 150 μm, and the particle size of W powder is 10 μm;
[0082] The rest of the settings are the same as those in Example 4.
[0083] The specific preparation process parameters and the composition of the obtained CrW alloy target are recorded in Table 1. The microstructure morphology of the obtained alloy is shown in Fig.10 middle.
[0084] Comparative Example 3
[0085] A method for preparing a CrW alloy target, which differs from Example 4 in that, step S1. Cr powder and W powder are mixed uniformly in a predetermined ratio, wherein the atomic ratio of W element in the predetermined ratio is 30%, the particle size of Cr powder is 25 μm, and the particle size of W powder is 45 μm;
[0086] The rest of the settings are the same as those in Example 4.
[0087] The specific preparation process parameters and the composition of the obtained CrW alloy target material are recorded in Table 1. The microstructure morphology of the obtained alloy is shown in Fig.11 middle.
[0088] Comparative Example 4
[0089] A method for preparing a CrW alloy target, which differs from Example 4 in that, step S1. Cr powder and W powder are mixed uniformly in a predetermined ratio, wherein the atomic ratio of W element in the predetermined ratio is 30%, the particle size of Cr powder is 150 μm, and the particle size of W powder is 45 μm;
[0090] The rest of the settings are the same as those in Example 4.
[0091] The specific preparation process parameters and the composition of the obtained CrW alloy target are recorded in Table 1. The microstructure morphology of the obtained alloy is shown in Fig.12 middle.
[0092] Table 1 Parameters and results of the preparation method of CrW alloy target in Examples 1-7 and Comparative Examples 1-4
[0093]
[0094] It can be seen from the data in Table 1 that the target material with the atomic ratio of up to 50% was prepared by optimizing the powder particle size and the molding process in Examples 1-7 of the present invention. Figure 2-8 It can be seen that the CrW alloy target of the present invention has good microstructure dispersion, uniform structure, no segregation, no agglomeration, etc., and a density of more than 99%. In addition, by comparing Comparative Example 1 with Example 1, although Comparative Example 1 uses 150μm Cr powder raw material, the added W content is less than 5%, which has little effect on its density. Both reach more than 99%, but the microstructures of the two are quite different, such as Figure 2 and Fig. 9 As shown, it can be seen that Fig. 9In Comparative Example 1, the dispersion of W in the Cr matrix is obviously poor.
[0095] By comparing Comparative Example 2 with Example 4, although Comparative Example 2 uses 150μm Cr powder as raw material, the density is greatly affected by the addition of W content reaching 30%. The density of Example 4 is 99.1%, while the density of Comparative Example 2 is only 98.3%. At the same time, the microstructures of the two are compared. Figure 5 and Fig.10 As shown, it can be seen that Fig.10 The dispersion of W in Comparative Example 2 is poor compared with that in Example 4.
[0096] By comparing Comparative Example 3 and Comparative Example 4, it is found that although both use 45μm W raw material, the Cr raw material is 25μm and 150μm respectively. The density of Comparative Example 3 and Comparative Example 4 is 98.9% and 98.1% respectively, which is very different. At the same time, both are less than the target value of 99%. Through the microstructure observation of the two, as shown in Fig.11 and Fig.12 As shown in the figure, it can be seen that this is mainly because the W particles are large and difficult to disperse in the Cr matrix, especially Fig.12 In Comparative Example 4, due to the large difference in particle sizes between W and Cr, W agglomeration is more obvious, resulting in a lower density after hot isostatic pressing.
[0097] In addition, through the comparison of Examples 3, 6, and 7, it can be found that the diffusion welding temperature has little effect on the final strength and welding rate of the diffusion welding, and excellent welding effects can be achieved within the process range of the present application.
Claims
1. A method for preparing a CrW alloy target, characterized in that: The specific steps include: S1. The Cr powder and the W powder are mixed uniformly in a predetermined ratio, wherein the atomic ratio of the W element in the predetermined ratio is 50%, the particle size of the Cr powder is 25 μm, and the particle size of the W powder is 10 μm; S2. The mixed powder is loaded into the encapsulation mold for degassing; S3. The degassed package is subjected to hot isostatic pressing; S4. The hot isostatic pressing process is followed by removing the jacket from the blank, and then cutting it into target pieces of the corresponding size, and grinding both end surfaces of the target piece; S5. Sandblasting the target plate at both ends after grinding. S6. The two end surfaces of the target sheet after sandblasting are electroplated; S7. The electroplated target sheet is stacked with an alloy backing plate of the same size and loaded into a sleeve mold for degassing; S8. The degassed package is subjected to diffusion welding; S9. Remove the sheath from the target sheet after diffusion welding, and then process it into a target material of a desired shape to obtain a CrW alloy target material with a backing plate. The CrW alloy target material has a density of more than 99%, and W is well dispersed in the Cr matrix, with a uniform structure, no segregation, and no agglomeration.
2. The preparation method according to claim 1, characterized in that In step S3, the processing temperature during the hot isostatic pressing process is 1200° C. to 1400° C. and the pressure is 100 to 150 MPa.
3. The preparation method according to claim 1, characterized in that: In step S4, after the grinding process, the flatness of both end surfaces of the target piece is less than 0.05 mm.
4. The preparation method according to claim 1, characterized in that: In step S5, after the sandblasting treatment, the roughness of both end surfaces of the target sheet is not less than Ra3.
6.
5. The preparation method according to claim 1, characterized in that: In step S8, the diffusion welding process is performed at a temperature of 500°C-950°C, a pressure of 100-150 MPa, and a heat preservation time of 3-6 hours.
6. A CrW alloy target material obtained by the preparation method according to any one of claims 1 to 5, characterized in that: The CrW alloy target material is composed of Cr and W in a predetermined ratio, wherein the atomic ratio of the W element is 50%.