Casting materials and casting methods for large wind power casting products

By adjusting the composition and process of the QT500-14 casting material to improve its low-temperature toughness and fatigue resistance, the problems of poor low-temperature toughness and fatigue fracture resistance of QT500-14 in the casting of large-scale wind power products have been solved, and the quality of the castings has been improved. Comprehensive performance and service life.

CN116200646BActive Publication Date: 2024-10-11SICHUAN MIRACLEYONGDA MASCH CO LDT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211736771.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-11
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

When using QT500-14 ductile cast iron to cast large-scale, thick-walled wind power products, there are problems such as poor low-temperature toughness and poor fatigue fracture resistance, which affects the performance and service life of wind power products.

Method used

By adjusting the component content of the casting material and the smelting preparation process, controlling the silicon content and the number of additions of pig iron to activate the molten iron, combined with spheroidization and inoculation treatment, the matrix structure is improved; the temperature and speed are controlled during the pouring process to optimize the sand mold and sand core Improve the structural strength and reduce the secondary expansion effect.

Benefits of technology

It improves the low-temperature impact performance and fatigue fracture resistance of casting materials, ensures the molding quality and service life of large-scale thick-walled wind power products, and is suitable for harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116200646B_ABST
    Figure CN116200646B_ABST
Patent Text Reader

Abstract

The invention discloses a casting material and a casting method for large-scale wind power casting products. Improvements are made in two aspects, namely, material composition and smelting preparation process. In the smelting preparation process, the silicon content of molten iron in the smelting step is controlled to control the composition of the obtained casting material. Meanwhile, pig iron is added twice in the smelting step to activate and purify the molten iron, thereby improving the purity of the molten iron and ensuring the stability of the molten iron composition before it is discharged from the furnace. This has an important promoting effect on the final mechanical properties and metallographic properties of the material, especially the low-temperature impact performance and fatigue performance of the material, so that the obtained casting material can have excellent comprehensive properties such as low-temperature impact resistance and fatigue fracture resistance, so that it can be used in the casting of large-scale thick-walled wind power products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of casting materials and processes, and in particular relates to a casting material and a casting method for large-scale wind power casting products. Background Art

[0002] With the development of large-scale wind turbines, the loads borne by major components are also increasing. The casting parts of wind turbines made of QT350-22AL and QT400-18AL materials have relatively low material strength. In order to meet their load requirements, the wall thickness, size and weight of the parts will inevitably increase, resulting in an increase in the cost of wind turbines and increasing the difficulty of assembling wind turbines. Therefore, the use of high-strength and high-toughness cast iron materials such as QT500-14 has become an important application direction for large-scale design of wind turbines. However, due to differences in material composition and other aspects, some casting defects such as shrinkage and shrinkage holes are easily caused during the casting process of these large and thick-walled castings of wind turbine products, affecting the performance of the castings. In terms of performance, although these high-strength and high-toughness cast iron materials such as QT500-14 have higher relative strength, they often have poor low-temperature toughness and poor fatigue fracture resistance, which affects the performance and service life of wind power products. Summary of the invention

[0003] The purpose of the present invention is to provide a casting material and a casting method for large wind power casting products, so as to solve the problems of poor low temperature toughness and poor fatigue fracture resistance when using QT500-14 ductile iron to cast large and thick-walled wind power products.

[0004] The present invention is achieved through the following technical solutions:

[0005] The casting materials used for large wind power casting products have the following components by weight:

[0006] C: 3.0-3.5%, Si: 3.3-3.5%, Mn < 0.20%, P < 0.035%, S < 0.012%, Sb: 0.004-0.005%, Mg: 0.035-0.045%, Cu < 0.04%, Cr < 0.035%, the rest is Fe;

[0007] The preparation steps of the casting material are as follows:

[0008] a. Smelting: The raw materials used for smelting include, by weight: pig iron: 40-60%, scrap steel: 10-30%, and recycled materials: 10-30%;

[0009] Pig iron, scrap steel and recycled materials are added into the furnace, 10% to 20% of the pig iron is reserved, and carburizer and ferrosilicon are added during the smelting process; the temperature is controlled at 1350 to 1390°C during the smelting process; after smelting for a period of time, the furnace is stopped and left to stand for a period of time to allow the oxidized slag in the furnace to fully float to the surface of the molten liquid, and the slag removal treatment is carried out. After the slag removal treatment is completed, the reserved pig iron is added into the furnace, and the temperature is raised again to the molten iron discharge temperature;

[0010] b. Spheroidizing and inoculating treatment: adding a rare earth-containing spheroidizing agent to one side of the bottom of the spheroidizing bag, and adding a high-barium inoculant and silicon steel sheets on the spheroidizing agent in sequence, wherein the amount of silicon steel sheets added is 0.6-0.8% of the weight of the molten iron, the amount of the high-barium inoculant is 0.15% of the weight of the molten iron, and the high-barium inoculant is a high-barium inoculant with a particle size of 8-15 mm;

[0011] The molten iron is poured into the spheroidizing ladle for spheroidization and inoculation. The spheroidizing temperature is 1420-1450℃ and the spheroidizing time is 2-3min.

[0012] When the molten iron is discharged from the furnace, an inoculant is thrown in. The inoculant is a silicon-barium inoculant with a particle size of 3-8 mm, and the amount of the silicon-barium inoculant thrown is 0.2-0.3% of the weight of the molten iron;

[0013] c. Pouring; during pouring, a flow-inoculating agent is added along with the molten iron, and the inoculating time of the flow-inoculating agent is the same as the time when the molten iron flows in; the flow-inoculating agent adopts a silicon-barium inoculant with a particle size of 0.2-0.7mm, and the amount of the flow-inoculating agent added is 0.15% of the weight of the molten iron.

[0014] As a further improvement to the above technical solution, the temperature of the molten iron out of the furnace in step a and step b is controlled to be 1470-1520°C.

[0015] As a further improvement to the above technical solution, when the molten iron is discharged from the furnace in step a, the silicon content in the molten iron is controlled to be 2.3-2.5%.

[0016] As a further improvement to the above technical solution, the pig iron uses high-purity pig iron or Q10 pig iron, and the scrap steel uses Class A scrap steel.

[0017] On the other hand, the present invention also relates to a casting method for casting a large wind power casting product, comprising the step of preparing a casting model before casting, and the preparation of the casting model comprises the following steps:

[0018] Modeling; the amount of resin in the molding sand used to prepare the sand mold is 1.2-1.4% of the weight of the molding sand, and the amount of curing agent is 35-50% of the resin, so that the strength of the sand mold reaches 4MPa-8MPa, and the sand tamping operation is performed during the sand operation;

[0019] Core making: When making the sand core, a core bone is set inside the sand core, and a ventilation rope is wound around the core bone and led out to the surface of the core head of the sand core; the amount of resin in the molding sand used to prepare the sand core is 1.2-1.4% of the weight of the molding sand, and the amount of curing agent is 35-50% of the amount of resin, so that the strength of the sand core reaches 4MPa-8MPa, and the sand tamping operation is performed during the sand operation;

[0020] Painting: Use high temperature resistant paint to paint the surface of sand mold and sand core, the paint concentration is 50-70 degrees Baume, and the coating thickness is 150-200um;

[0021] After the box is closed, a counterweight is used to press the box. The weight of the counterweight used to press the box is 5-8 times the weight of the poured molten iron.

[0022] As a further improvement to the above technical solution, during pouring, the pouring temperature is controlled to be 1300-1330°C.

[0023] As a further improvement to the above technical solution, the pouring speed is controlled and the pouring time is controlled within 200s.

[0024] As a further improvement to the above technical solution, the time from spheroidization of the casting material to the end of pouring is controlled within 25 minutes, preferably within 10 minutes.

[0025] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0026] By making improvements in both material composition and smelting preparation process, in the smelting preparation process, the silicon content of the molten iron in the smelting step is controlled, and the composition of the resulting casting material is controlled. At the same time, pig iron is added twice in the smelting step to activate and purify the molten iron, thereby improving the purity of the molten iron and ensuring the stability of the molten iron composition before it is fired. This has an important promoting effect on the final mechanical properties, metallographic properties, especially the low-temperature impact performance and fatigue performance of the material, so that the resulting casting material can have excellent comprehensive properties such as resistance to low-temperature impact and fatigue fracture, so that it can be used in the casting of large thick-walled wind power products.

[0027] In the spheroidizing, inoculating and pouring steps, by controlling the spheroidizing temperature / time, the components / addition amount of the spheroidizing inoculant / flow-inoculating agent and other preparation parameters, the matrix structure of the casting material is further improved, so that the matrix structure of the obtained casting material is finer and the graphite spheroidization is more rounded, thereby improving the comprehensive performance of the casting material.

[0028] At the same time, the study found that when using this casting material for casting, the secondary expansion effect of the material is obvious, which has a great impact on the molding quality of large-scale wind power products; based on this problem, by improving the structural strength of the sand mold and sand core in the casting model, it is controlled within a certain strength range, and at the same time the pouring temperature and pouring speed of the molten iron are controlled, which solves the problem of secondary expansion of the casting material during the pouring process and ensures the comprehensive performance of the final cast wind power products. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0030] Figure 1a ) is the metallographic structure diagram of the sample before corrosion at a thickness of 150 mm in an embodiment of the present invention.

[0031] Figure 1b ) is the metallographic structure diagram of the sample after corrosion at a thickness of 150 mm in an embodiment of the present invention.

[0032] Figure 2a ) is the metallographic structure diagram of the sample before corrosion at a thickness of 200 mm in an embodiment of the present invention.

[0033] Figure 2b ) is the metallographic structure diagram of the sample after corrosion at a thickness of 200 mm in an embodiment of the present invention.

[0034] Figure 3a ) is a schematic diagram of the metallographic structure of the sample before corrosion at a thickness of 250 mm in an embodiment of the present invention.

[0035] Figure 3b ) is a schematic diagram of the metallographic structure of the sample after corrosion at a thickness of 250 mm in an embodiment of the present invention.

[0036] Figure 4 This is a front view of the wind turbine base structure cast in the present invention.

[0037] Figure 5 This is a top view of the wind turbine base structure cast in the present invention. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0039] Wind power casting products are usually large in size, thick in wall and complex in structure, which brings great difficulties to the casting and molding quality of wind power product castings. Casting defects in the casting process will seriously affect the performance and service life of the castings. Therefore, improving the casting process of wind power product castings and improving the performance of casting raw materials are important research directions to improve the performance of wind power product castings.

[0040] Based on the demand for structural strength of casting products, since QT500 series cast iron is superior to QT400 series in comprehensive performance, a lot of research has been carried out on the use of QT500 materials to cast wind power products, including research on QT500-14 materials. At present, most of the research on QT500-14 materials focuses on the mechanical strength and metallographic structure of the materials at room temperature. However, due to the use and installation environment requirements of wind power products, the low-temperature performance of the materials, especially the toughness of the materials in low-temperature environments, is also an important indicator affecting the performance of wind power products. The existing QT500-14 materials generally have the problem of low impact performance in low-temperature environments (such as -30°C).

[0041] At the same time, as the operating environment of wind power products becomes increasingly harsh, wind power mainframe manufacturers are currently putting forward higher requirements on the performance of wind power products. One of them is the material's fatigue fracture resistance. Tests have shown that the material's fatigue fracture resistance has an important impact on the product's service life and is an important indicator for evaluating the quality and performance of wind power products.

[0042] Since wind power products are large in size and have thicker walls (the wall thickness at the thickest position can reach more than 200mm), the casting process originally suitable for QT400-18 materials is often not directly applicable to the casting of QT500-14 materials. Therefore, it is necessary to adjust the casting process of the casting according to the relevant casting performance characteristics of the material.

[0043] Usually, the research on a cast iron material usually involves two aspects: material composition and material smelting method. Both the material composition and the smelting of the material will have a great impact on the final performance of the material. Specifically in this embodiment, certain adjustments and optimizations are made to the key elements in the casting material.

[0044] Among them, the component contents by weight are as follows: C: 3.0-3.5%, Si: 3.3-3.5%, Mn<0.20%, P<0.035%, S<0.012%, Sb: 0.004-0.005%, Mg: 0.035-0.045%, Cu<0.04%, Cr<0.035%, and the rest is Fe.

[0045] The C content in QT500-14 has a great influence on the spheroidization effect, material properties and casting properties. By increasing the C content in the composition, more graphite is precipitated. At the same time, by controlling the smelting preparation parameters, a large number of dispersed graphite balls are formed in the material, and the size of the graphite balls is smaller and the roundness is better, thereby improving the comprehensive performance of the material. In addition, during the casting process, the higher carbon content in the material can well reduce the shrinkage volume, make the molded castings more dense, and improve the casting quality of the castings.

[0046] The Si content in QT500-14 is controlled. Si does not form carbide elements and promotes graphite spheroidization. At the same time, Si can increase the eutectic temperature and reduce the carbon content of the eutectic. Combined with the inoculation effect of Si in QT500-14, the ratio of pearlite and ferrite in the material changes, promoting the production of ferrite, thereby improving the final performance of the material.

[0047] By controlling the Sb content in QT500-14 and keeping the Sb content within a very small range, the study found that the casting material within this range can have finer grains in terms of material matrix structure and better graphite morphology, thereby effectively improving the material's strength, resistance to low-temperature impact, and resistance to fatigue fracture.

[0048] Accordingly, the smelting preparation process of the casting material is as follows:

[0049] a. Smelting;

[0050] The raw materials used in smelting include, by weight: pig iron: 40-60%, scrap steel: 10-30%, and recycled materials: 10-30%; the pig iron uses high-purity pig iron or Q10 pig iron, and the scrap steel uses Class A scrap steel to improve the stability of the molten iron composition;

[0051] First, pig iron, scrap steel and recycled materials are added into the furnace. In this step, 10% to 20% of the pig iron is reserved, and carburizer and ferrosilicon are added during the smelting process.

[0052] The smelting temperature during the smelting process is controlled at 1350-1390°C;

[0053] After smelting for a period of time, stop the furnace and let it stand for 5-10 minutes to allow the oxidized slag in the furnace to fully float to the surface of the molten liquid, remove the oxidized slag on the surface of the molten liquid, and then add the previously reserved pig iron into the furnace, and raise the temperature again to the molten iron discharge temperature. In the smelting process, pig iron is added in two steps. In the second stage of smelting, adding pig iron can activate the molten iron and purify the purity of the molten iron, thereby ensuring the stability of the material components and making it easy to control the material components;

[0054] In this step, the chemical composition of the molten iron is tested before it is taken out of the furnace to ensure that the silicon content in the molten iron is 2.3-2.5% when the molten iron is taken out of the furnace;

[0055] b. Spheroidization and inoculation treatment;

[0056] Prepare a spheroidizing bag, add a spheroidizing agent containing rare earth on one side of the bottom of the spheroidizing bag, and add a high-barium inoculant and silicon steel sheets on the spheroidizing agent in sequence, wherein the amount of silicon steel sheets added is 0.6-0.8% of the weight of the molten iron, the amount of high-barium inoculant is 0.15% of the weight of the molten iron, and the high-barium inoculant has a particle size of 8-15 mm;

[0057] The molten iron is taken out of the furnace and poured into the spheroidizing ladle for spheroidization and inoculation. The spheroidizing temperature is 1420-1450℃ and the spheroidizing time is 2-3min.

[0058] When the molten iron is discharged from the furnace, an inoculant is thrown in. The inoculant is a silicon-barium inoculant with a particle size of 3-8 mm, and the amount of the silicon-barium inoculant thrown is 0.2-0.3% of the weight of the molten iron;

[0059] Among them, the temperature of molten iron out of the furnace is controlled at 1470~1520℃;

[0060] c. Pouring;

[0061] Before pouring, the molten iron is deslagging to remove the oxide slag on the surface of the molten iron. After deslagging, the molten iron is left to stand for 2-3 minutes to allow the residue in the spheroidizing bag to fully float to the surface of the molten iron. The deslagging operation is performed again, the molten iron temperature is measured and preparations are made for transfer and pouring;

[0062] Silicate cotton is spread on the surface of the molten iron to further filter the residue in the molten iron, the temperature of the molten iron is measured to control the pouring temperature at 1300-1330°C, and a flow-inoculating agent is added above the pouring cup along with the molten iron during pouring, and the adding speed of the flow-inoculating agent is controlled so that the adding time of the flow-inoculating agent is roughly the same as the pouring time of the molten iron, so as to avoid that the molten iron is not completely poured when the flow-inoculating agent is added; the flow-inoculating agent adopts a silicon-barium inoculant with a particle size of 0.2-0.7mm, and the adding amount of the flow-inoculating agent is 0.15% of the weight of the molten iron;

[0063] The time from spheroidization to the end of pouring should be controlled within 25 minutes, preferably within 10 minutes.

[0064] During the pouring process, ignition rods are used to draw air from each pouring riser and parting position to fully discharge the gas in the mold cavity.

[0065] In the study of the pouring performance of QT500-18, it was found that QT500-18 has a secondary expansion problem during the pouring process, which directly affects the molding quality of the casting. In order to solve the impact of this problem on casting, the casting process was improved accordingly.

[0066] With regard to the casting process, the preparation process of the casting model is first improved, including the following steps:

[0067] a. Modeling;

[0068] The mold for preparing the sand mold includes a cover box and a bottom box. After the mold is placed in a flat position, the mold is installed to prepare the sand mold; in the molding sand used for preparing the sand mold, the content of resin is controlled to be 1.2-1.4% of the weight of the molding sand, the content of curing agent is controlled to be 35-50% of the weight of the resin, and the strength of the sand mold is controlled to be 4MPa-8MPa;

[0069] During the sand mold preparation process, a wooden stick is used to tamp the sand during the sand feeding operation to make the sand mold compact.

[0070] The ceramic tube in the sand mold is placed at the bottom. The riser vent is set at the top of the casting casting model so that the molten iron can be fully deslagging when pouring. A vent with a diameter of 200mm is set at the corresponding sand core position on the cover box in the mold to facilitate sufficient exhaust inside the model cavity.

[0071] b. Core making;

[0072] When making the sand core, a core bone is set inside the sand core, and a ventilation rope is wound around the core bone and led out to the surface of the core head of the sand core; a ventilation rope is set on the core bone and led to the exhaust position of the core head at the bottom of the sand core, which can effectively improve the exhaust capacity of the sand core and also plays an important role in improving the secondary expansion effect;

[0073] In the molding sand used to prepare the sand core, the content of resin is controlled to be 1.2-1.4% of the weight of the molding sand, the content of curing agent is controlled to be 35-50% of the weight of the resin, and the strength of the sand core is controlled to be 4MPa-8MPa;

[0074] During the sand core preparation process, a wooden stick is used to tamp the sand to make the sand core compact.

[0075] In the process of preparing sand molds and sand cores, the content of resin and curing agent in the sand is controlled to improve the structural strength of the sand molds and sand cores, avoid the damage of the sand molds and sand cores due to the secondary expansion of QT500-14 during the casting process, and improve the molding quality of castings. Since the increase of resin and curing agent content in the sand will affect the fluidity of the sand, wooden sticks are used to tamp the sand during the sand operation of the sand mold and sand core preparation to make the internal structure of the sand mold and sand core more compact.

[0076] c. Painting;

[0077] The surface of the sand mold and sand core is painted with a paint that is resistant to high temperatures of 1410-1470°C. The paint concentration is controlled at 50-70 degrees Baume, and the coating thickness is 150-200um.

[0078] d. Close the box;

[0079] Place the sand mold on the sand bed, place the sand core in the correct position in the sand mold, and perform the box closing operation;

[0080] After the box is assembled, a counterweight is used to press the box. The weight of the counterweight used to press the box is 5-8 times the weight of the poured molten iron.

[0081] At this point, the preparation of the pouring model is completed, and then the pouring operation is carried out. During pouring and molding, the pouring temperature is controlled to be 1300-1330°C, and the pouring speed is controlled to achieve rapid pouring and molding. The pouring time is controlled within 200s to reduce the influence of the secondary expansion effect of the material on the casting quality.

[0082] By improving the casting model preparation process and the casting process, the problem of using Q500-14 material to cast large thick-walled wind power castings, which causes a large secondary expansion effect due to the large material pouring amount, thus affecting the casting quality, has been well solved.

[0083] Under different casting thickness conditions, the relevant properties of the casting material are tested, as follows:

[0084] Example 1

[0085] a. Smelting: The raw materials used for smelting include, by weight: pig iron: 50%, scrap steel: 30%, and recycled materials: 20%;

[0086] First, add pig iron, scrap steel and recycled materials into the furnace. In this step, reserve 10% of the pig iron. Add carburizer and ferrosilicon during the smelting process. The smelting temperature is controlled at 1350°C. After smelting for a period of time, stop the furnace and let it stand for 5 minutes to allow the slag in the furnace to fully float to the surface of the melt. Remove the slag on the surface of the melt, and then add the reserved pig iron into the furnace and raise the temperature to 1470°C again.

[0087] Detect the chemical composition of molten iron before it comes out of the furnace:

[0088] C: 3.65%, Si: 2.40%, Mn<0.097%, P<0.011%, S<0.033%, Sb: 0.0015%, Mg: 0.0006%, Cu<0.031%, Cr<0.014%.

[0089] b. Spheroidizing and inoculating treatment; preparing a spheroidizing bag, adding a spheroidizing agent containing rare earth to one side of the bottom of the spheroidizing bag, adding a high-barium inoculant with a particle size of 8-15mm and a certain amount of silicon steel sheets on the spheroidizing agent, the amount of silicon steel sheets added is 0.6% of the weight of the molten iron, and the amount of high-barium inoculant is 0.15% of the weight of the molten iron; taking the molten iron out of the furnace, pouring it into the spheroidizing bag, and carrying out spheroidizing and inoculating in the bag; the spheroidizing treatment temperature is 1420℃, the spheroidizing time is 3min, and the time from spheroidizing treatment to the end of pouring is 9min; during the process of tapping the molten iron, the broth is thrown, and a silicon-barium inoculant with a particle size of 3-8mm is added, and the throwing amount of the silicon-barium inoculant is 0.3% of the weight of the molten iron; wherein, the furnace temperature of the molten iron spheroidizing treatment is controlled at 1470℃.

[0090] c. Pouring; measuring the temperature of the molten iron, controlling the pouring temperature at 1323°C, adding a flow inoculant along with the molten iron above the pouring cup during pouring, and the pouring time is 28s; the flow inoculant uses a 0.15% silicon-barium inoculant with a particle size of 0.2-0.7mm, wherein the amount of the flow inoculant added is 0.15% of the weight of the molten iron.

[0091] The chemical composition of the casting material obtained by smelting is as follows:

[0092] C: 3.130%, Si: 3.380%, Mn<0.110%, P<0.017%, S<0.0090%, Sb: 0.004%, Mg: 0.044%, Cu<0.010%, Cr<0.019%.

[0093] The smelted material was used to cast sample test blocks at thicknesses of 150mm, 200mm and 250mm. The mechanical properties of the test blocks were tested as follows: (The testing standards are in accordance with GB / T228.1-2010 and GB / T229-2020 respectively)

[0094]

[0095]

[0096] The metallographic properties of the samples at the above thickness positions were tested, and the test results are as follows: (Testing standard is in accordance with GB / T9441-2009)

[0097] Sample with thickness of 150mm:

[0098] The pearlite content in the matrix is ​​less than 3%, the cementite is less than 0.5%, the ferrite content is greater than 95%, the spheroidization level is 2, the graphite ball size is 6-8, the graphite ball spheroidization rate (graphite form V+VI) is 95%, and the number of graphite balls with a graphite ball spheroidization rate of 95% is 180-185 / mm 2 ;like Figure 1a ), Figure 1b ) as shown.

[0099] Sample with thickness of 200mm:

[0100] The pearlite content in the matrix is ​​less than 3%, the cementite is less than 0.5%, the ferrite content is greater than 95%, the spheroidization level is 2, the graphite ball size is 6 to 8, the graphite ball spheroidization rate (graphite form V+VI) is 95%, and the number of graphite balls with a graphite ball spheroidization rate of 95% is 200-250 / mm 2 ;like Figure 2a ), Figure 2b ) as shown.

[0101] Sample with thickness of 250mm:

[0102] The pearlite content in the matrix is ​​less than 3%, the cementite is less than 0.5%, the ferrite content is greater than 95%, the spheroidization level is 2, the graphite ball size is 6 to 8, the graphite ball spheroidization rate (graphite form V+VI) is 95%, and the number of graphite balls with a graphite ball spheroidization rate of 95% is 200-250 / mm 2 ;like Figure 3a ), Figure 3b ) as shown.

[0103] The fatigue performance test was carried out on the samples at the above thickness positions to test their metallographic properties. The test results are as follows:

[0104]

[0105]

[0106] It can be seen from the above test data that the room temperature mechanical properties, low temperature impact properties, metallographic properties and fatigue properties (including fatigue fracture, -30℃ fracture toughness, fatigue crack extension threshold) of the materials at different wall thickness positions all meet the requirements of the corresponding standards, indicating that the prepared QT500-14 has good comprehensive performance in casting large wind power products and can be widely used in the casting of large wind power products. The prepared material has higher strength, finer matrix structure and higher hardness (HB160-210). While ensuring the structural strength of the product, the weight of the product is reduced and the service life of the product is increased. The service life of the product can reach 20-30 years (the service life of QT400-18 material castings is generally 15-20 years); and due to its good low-temperature toughness and low-temperature fatigue performance, it can be used in harsh environments such as low temperature and severe cold.

[0107] Example 2

[0108] By pouring Figure 4 and5 Take the wind turbine base shown as an example.

[0109] Preparing a casting model for casting a wind turbine base includes the following steps:

[0110] Modeling; the amount of resin in the molding sand used to prepare the sand mold is 1.4% of the weight of the molding sand, the amount of curing agent is 50% of the amount of resin, and the sand tamping operation is performed during the sand operation. The strength of the prepared sand mold is 7.2MPa;

[0111] Core making: When making the sand core, a core bone is set in the sand core, and a ventilation rope is wound around the core bone and led out to the surface of the core head of the sand core; the amount of resin in the molding sand used to prepare the sand core is 1.4% of the weight of the molding sand, and the amount of curing agent is 50% of the amount of resin. The sand is tamped during the sand operation, and the strength of the prepared sand core is 6.9MPa;

[0112] Painting: Use high temperature resistant paint to paint the surface of sand mold and sand core, the paint concentration is 70 degrees Baume, and the coating thickness is 200um;

[0113] After the box is closed, a counterweight is used to press the box. The weight of the counterweight used to press the box is 8 times the weight of the poured molten iron.

[0114] The molten iron in Example 1 was used for casting to obtain a wind turbine base, and the appearance quality of the wind turbine base was tested, and the appearance quality met customer requirements; NDT flaw detection (ultrasonic, magnetic powder) was performed on the wind turbine base, and no obvious defects such as looseness and shrinkage holes were found, and the performance met customer quality requirements.

[0115] The performance of the samples pre-set at the casting parting position or designated position is tested, and the relevant mechanical properties (including low-temperature impact properties) and metallographic properties meet the standard requirements.

[0116] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the definition of the attached claims.

[0117] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.

[0118] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0119] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.

Claims

1. Casting material for large wind power casting products, characterized in that: The components by weight are as follows: C: 3.0-3.5%, Si: 3.3-3.5%, Mn < 0.20%, P < 0.035%, S < 0.012%, Sb: 0.004-0.005%, Mg: 0.035-0.045%, Cu < 0.04%, Cr < 0.035%, the rest is Fe; The preparation steps of the casting material are as follows: a. Smelting: The raw materials used for smelting include, by weight: pig iron: 40-60%, scrap steel: 10-30%, recycled materials: 10-30%; Pig iron, scrap steel and recycled materials are added into the furnace, 10% to 20% of the pig iron is reserved, and carburizer and ferrosilicon are added during the smelting process; the temperature is controlled at 1350 to 1390°C during the smelting process; after smelting for a period of time, the furnace is stopped and left to stand for a period of time to allow the oxidized slag in the furnace to fully float to the surface of the molten liquid, and the slag is removed. After the slag removal is completed, the reserved pig iron is added into the furnace and the temperature is raised again to the temperature at which the molten iron is discharged from the furnace; b. Spheroidizing and inoculating treatment: adding a rare earth-containing spheroidizing agent to one side of the bottom of the spheroidizing bag, and adding a high-barium inoculant and silicon steel sheets on the spheroidizing agent in sequence. The amount of silicon steel sheets added is 0.6-0.8% of the weight of the molten iron, and the amount of high-barium inoculant is 0.15% of the weight of the molten iron. The high-barium inoculant has a particle size of 8-15 mm. The molten iron is poured into the spheroidizing ladle for spheroidization and inoculation. The spheroidizing temperature is 1420-1450℃ and the spheroidizing time is 2-3min. When the molten iron is taken out of the furnace, the inoculant is thrown. The inoculant is a silicon-barium inoculant with a particle size of 3-8 mm. The amount of the silicon-barium inoculant thrown is 0.2-0.3% of the weight of the molten iron. c. Pouring: During pouring, a flow-inoculating agent is added along with the molten iron, and the inoculation time of the flow-inoculating agent is the same as the molten iron inflow time; the flow-inoculating agent adopts a silicon-barium inoculant with a particle size of 0.2-0.7mm, and the amount of the flow-inoculating agent added is 0.15% of the weight of the molten iron.

2. The casting material for large wind power casting products according to claim 1, characterized in that: In step a and step b, the temperature of the molten iron out of the furnace is controlled to be 1470-1520°C.

3. The casting material for large wind power casting products according to claim 1, characterized in that: When the molten iron is discharged from the furnace in step a, the silicon content in the molten iron is controlled to be 2.3-2.5%.

4. The casting material for large-scale wind power casting products according to claim 1, characterized in that: The pig iron used is high-purity pig iron or Q10 pig iron, and the scrap steel used is Class A scrap steel.

5. A casting method for casting a large wind power casting product using the casting material described in claim 1, characterized in that: The method comprises the steps of preparing a casting model before casting, wherein the preparation of the casting model comprises the following steps: Modeling; the amount of resin in the molding sand used to prepare the sand mold is 1.2-1.4% of the weight of the molding sand, and the amount of curing agent is 35-50% of the resin, so that the strength of the sand mold reaches 4MPa-8MPa, and the sand tamping operation is performed during the sand operation; Core making: When making the sand core, a core bone is set inside the sand core, and a ventilation rope is wound around the core bone and led out to the surface of the sand core head; the amount of resin in the molding sand used to prepare the sand core is 1.2-1.4% of the weight of the molding sand, and the amount of curing agent is 35-50% of the amount of resin, so that the strength of the sand core reaches 4MPa-8MPa, and the sand tamping operation is performed during the sand operation; Painting: Use high temperature resistant paint to paint the surface of sand mold and sand core, the paint concentration is 50-70 degrees Baume, and the coating thickness is 150-200um; After the box is closed, a counterweight is used to press the box. The weight of the counterweight used to press the box is 5-8 times the weight of the poured molten iron.

6. The casting method for casting a large wind power casting product according to claim 5, characterized in that: During pouring, the pouring temperature is controlled at 1300-1330°C.

7. The casting method for casting a large wind power casting product according to claim 5, characterized in that: Control the pouring speed and keep the pouring time within 200s.

8. The casting method for casting a large wind power casting product according to claim 5, characterized in that: The time from spheroidization of casting materials to the end of pouring is controlled within 25 minutes.

9. The casting method for casting a large wind power casting product according to claim 8, characterized in that: The time from spheroidization of casting materials to the end of pouring is controlled within 10 minutes.