Alumina-supported copper heterogeneous catalyst with molecular imprinting function and preparation method and application thereof
By performing temperature-programmed adsorption technology on alumina-supported copper catalysts to adsorb template molecules and organic ligands, the problem of difficulty in balancing activity and selectivity of existing catalysts was solved, and efficient hydrogenation of nitro compounds was achieved with repeatability. usability.
Patent Information
- Application Number
- CN202310193937.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-03-03
AI Technical Summary
Existing catalysts usually sacrifice activity when improving selectivity, making it difficult to achieve high activity conversion based on the original reaction, and cannot accurately control selectivity, which limits the development of catalysts.
Alumina-loaded copper heterogeneous catalyst is used, and the alumina carrier, copper salt and water are mixed for reduction deposition, and then roasted and reduced. Combined with programmed temperature adsorption technology, the template molecules and organic ligands are adsorbed to the surface of the catalyst to form a Molecularly imprinted functional catalysts.
It achieves high activity and selectivity in the hydrogenation reaction of nitro compounds while improving the molecular imprinting effect of the catalyst. The catalyst is easy to separate from reactants and products, is reusable, and is suitable for industrial applications.
Smart Images

Figure CN116212873B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials and catalysts, and in particular to an alumina-supported copper heterogeneous catalyst with molecular imprinting function, and a preparation method and application thereof. Background Art
[0002] Selectivity is an important indicator of catalyst performance, and improving the selectivity of heterogeneous catalysts has also become one of the research topics that has attracted much attention in the field of catalysis. In recent years, many catalytic materials and methods have been developed to improve the selectivity of heterogeneous reactions, including surface-modified catalysts, new nanostructured catalysts, self-assembled materials, metal alloys, and single-atom catalysts. Among them, molecular imprinting technology containing specific recognition sites is considered to be a more effective method. Due to the advantages of molecular imprinting technology such as specific recognition, predictable structure, controllable preparation, and wide application, this technology has been increasingly favored in the fields of chromatographic separation, chemical sensors, and biological binding analysis, especially in the field of catalysis. At present, molecular imprinting technology in the field of heterogeneous catalysis is mainly divided into two types, namely, using transition metals such as titanium dioxide and cobalt tetraoxide to cover redundant active sites or using organic molecules such as long-chain aliphatic hydrocarbons, sulfides, and amines to poison some active sites to achieve high selectivity and molecular imprinting function for specific types of reactions. However, these methods mostly sacrifice the activity of the catalyst while improving selectivity, and do not create new active sites. It is difficult to achieve high-activity conversion of new reactions, and can only improve selectivity on the basis of the original catalytic reaction, which greatly limits its development. Catalyst surface modification is one of the effective methods to improve catalyst activity, but this method cannot precisely control the selectivity of the catalyst. Therefore, it is of great significance to create a new type of active site during the surface modification process and prepare a heterogeneous catalyst that has both high catalytic activity and high selectivity.
[0003] Generally speaking, nitrogen-containing complexes have the advantages of a wide variety, diverse structures, easy coordination with metals, and good solubility, and are often used as ligands for catalyst surface modification to improve catalyst activity. However, in the process of catalyst surface modification, there are no reports of cases where the reaction substrate is used as a template molecule and a placeholder molecule to regulate the binding site and modification effect of the ligand to achieve high catalyst activity and molecular imprinting function. Summary of the invention
[0004] In view of this, the present invention provides an alumina-supported copper heterogeneous catalyst with molecular imprinting function and a preparation method and application thereof. The catalyst provided in the present application is applied to the hydrogenation reaction of nitro compounds, and has high hydrogenation activity and good selectivity.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] A method for preparing an alumina-supported copper heterogeneous catalyst having a molecular imprinting function comprises the following steps:
[0007] The aluminum oxide carrier, copper salt, water and reducing agent are mixed for reduction deposition, and the obtained reduction deposition product is sequentially calcined and reduced to obtain an aluminum oxide-supported copper precursor;
[0008] The template molecule and the organic ligand are sequentially adsorbed into the alumina-supported copper precursor by a programmed temperature adsorption method to obtain an alumina-supported copper heterogeneous catalyst with molecular imprinting function; the template molecule is a nitro compound.
[0009] Preferably, the method for preparing the alumina carrier comprises: mixing an aluminum salt solution and an alkaline solution to perform a precipitation reaction to obtain an aluminum hydroxide gel; and sequentially aging, washing, drying and calcining the aluminum hydroxide gel to obtain the alumina carrier.
[0010] Preferably, the copper salt includes one or more of copper chloride, nitrate, sulfate and acetate; the copper loading in the alumina-loaded copper precursor is 0.1 to 10 wt%;
[0011] The reducing agent is one or more of sodium borohydride, sodium hydride, lithium aluminum tetrahydride, hydrazine hydrate, phenylsilane, formaldehyde, citric acid, sodium citrate and vitamin C; the molar ratio of the reducing agent to the copper salt is 1:(1-10); the temperature of the reduction deposition is 20-80°C;
[0012] The reduction deposition method comprises: firstly mixing the alumina carrier, copper salt and water, then adding a reducing agent, adjusting the pH value of the reaction solution to 11-14 using an alkaline solution 0-30 minutes after adding the reducing agent, and then depositing at 20-80°C for 2-8 hours.
[0013] Preferably, the calcination temperature is 200-500°C, the time is 2-10h, and the heating rate to the calcination temperature is 2-10°C / min;
[0014] The reduction is carried out in a reducing gas, the volume fraction of hydrogen in the reducing gas is 5 to 100%; the flow rate of the reducing gas is 5 to 20 mL / min; the reduction temperature is 250 to 450° C., the reduction time is 2 to 6 hours, and the heating rate to the reduction temperature is 2 to 10° C. / min.
[0015] Preferably, the method of sequentially adsorbing the template molecule and the organic ligand into the alumina-loaded copper precursor by means of programmed temperature adsorption comprises: placing the template molecule in the middle and upper reaches of a tubular furnace, placing the alumina-loaded copper precursor in the middle and lower reaches of the tubular furnace, performing a first temperature increase adsorption, then placing the organic ligand in the middle and upper reaches of the tubular furnace, and placing the alumina-loaded copper precursor adsorbed with the template molecule in the middle and lower reaches of the tubular furnace for a second temperature increase adsorption; the temperature of the first temperature increase adsorption is 50 to 300°C, the insulation time is 0.5 to 5h, and the heating rate of heating to the temperature of the first temperature increase adsorption is 0.5 to 10°C / min; the temperature of the second temperature increase adsorption is 50 to 250°C, the insulation time is 0.5 to 5h, and the heating rate of heating to the temperature of the second temperature increase adsorption is 0.5 to 10°C / min.
[0016] Preferably, the template molecule is one of nitrobenzene and its derivatives, nitronaphthalene and its derivatives, nitropyrene and its derivatives;
[0017] The organic ligand is one of pyridine and its derivatives, bipyridine and its derivatives, or phenanthroline and its derivatives.
[0018] Preferably, the structure of the template molecule is a structure shown in any one of Formulas 1 to 3:
[0019]
[0020] In formulas 1 to 3: R 1 , R 2 and R 3 are independently hydrogen, -(C1-C 12 )-alkyl, -(C3-C 12 )-cycloalkyl, -(C3-C 12 )-heterocycloalkyl, (C6-C 20 )-aryl, (C3-C 20 )-heteroaryl, -O-(C1-C 12 )-alkyl, -O-(C3-C 12 )-cycloalkyl, phenoxy, halogen, trifluoromethyl, hydroxyl, amino or nitro; wherein n is 1 to 5, and n R 1 The groups are the same or different; in formula 2: n is 1 to 7, and n R 1 The groups are the same or different; in formula 3: n is 1 to 9, and n R 3 The groups are the same or different;
[0021] The structure of the organic ligand is any one of formulas 4 to 12:
[0022]
[0023]
[0024] In formula 4 to formula 12: R 4 , R 5 , R 6 and R 7 is hydrogen, -(C1-C 12 )-alkyl, -O-(C1-C 12 )-alkyl, halogen, trifluoromethyl, hydroxyl or amine; in Formula 4: n is 1 to 5, and n R 1 The groups are the same or different; in Formula 5, Formula 7, Formula 8, Formula 10 and Formula 11, n is independently 1 to 4, m is independently 1 to 4, and n R 5 The groups are the same or different, m R 6 The groups are the same or different; in Formula 6, Formula 9 and Formula 12, n is independently 1 to 8, and n R 7 The groups may be the same or different.
[0025] The present invention also provides an alumina-supported copper heterogeneous catalyst with molecular imprinting function prepared by the preparation method described in the above scheme, comprising an alumina carrier, copper supported on the alumina carrier, and template molecules and organic ligands adsorbed on the alumina carrier.
[0026] The present invention also provides the use of the alumina-supported copper heterogeneous catalyst with molecular imprinting function described in the above scheme in catalyzing the hydrogenation reaction of nitro compounds.
[0027] Preferably, the nitro compound includes one or more of nitrobenzene and its derivatives, nitronaphthalene and its derivatives, and nitropyrene and its derivatives.
[0028] The present invention provides a method for preparing an alumina-supported copper heterogeneous catalyst with molecular imprinting function, comprising the following steps: mixing an alumina carrier, a copper salt, water and a reducing agent for reduction deposition, calcining and reducing the obtained reduction deposition product in sequence to obtain an alumina-supported copper precursor; adsorbing a template molecule and an organic ligand into the alumina-supported copper precursor by a temperature-increasing adsorption method to obtain an alumina-supported copper heterogeneous catalyst with molecular imprinting function; the template molecule is a nitro compound. The present invention first prepares an alumina-supported copper precursor, and then uses a template molecule and an organic ligand to perform surface modification on the alumina-supported copper precursor, which can not only improve the hydrogenation activity and selectivity of the same type of nitro compounds, but also realize selective hydrogenation between different types of nitro compounds to achieve a molecular imprinting effect. In addition, the multiphase catalyst prepared by the present invention has an obvious molecular imprinting effect, is easy to separate from reactants and products, and can be reused, providing a new suitable industrial technology for the efficient and selective hydrogenation reaction of nitro compounds. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Schematic diagram of the continuous temperature increase adsorption process in the present invention;
[0030] Figure 2 The characterization results of alumina-supported copper heterogeneous catalyst with molecular imprinting function, including: (a) TGA graph, (b) infrared diffuse reflectance spectrum. DETAILED DESCRIPTION
[0031] The present invention provides a method for preparing an alumina-supported copper heterogeneous catalyst having a molecular imprinting function, comprising the following steps:
[0032] The aluminum oxide carrier, copper salt, water and reducing agent are mixed for reduction deposition, and the obtained reduction deposition product is sequentially calcined and reduced to obtain an aluminum oxide-supported copper precursor;
[0033] The template molecule and the organic ligand are sequentially adsorbed into the alumina-supported copper precursor by a programmed temperature adsorption method to obtain an alumina-supported copper heterogeneous catalyst with molecular imprinting function; the template molecule is a nitro compound.
[0034] First, the preparation method of the alumina carrier is described:
[0035] In the present invention, the preparation method of the alumina carrier preferably includes: mixing an aluminum salt solution and an alkaline solution for precipitation reaction to obtain an aluminum hydroxide gel; washing, drying and calcining the aluminum hydroxide gel in sequence (recorded as the first calcination) to obtain the alumina carrier. In the present invention, the aluminum salt is preferably one of aluminum trichloride and aluminum nitrate; the concentration of the aluminum salt solution is preferably 0.05-0.15 mol / L; the alkali in the alkaline solution is preferably at least one of potassium hydroxide, sodium hydroxide, potassium carbonate, potassium bicarbonate, sodium carbonate, sodium bicarbonate and ammonia water; the concentration of the alkaline solution is preferably 0.5-1 mol / L; the molar ratio of the aluminum salt and the alkali is preferably 1:(1-5); the volume ratio of the aluminum salt solution and the alkaline solution is preferably (3-10):1; in a specific embodiment of the present invention, the alkaline solution is preferably added dropwise to the aluminum salt solution; the temperature of the precipitation reaction is preferably 20-80°C, more preferably 25-50°C, The precipitation reaction time is preferably 2 to 8 hours, more preferably 4 to 6 hours, and the precipitation reaction time is counted from the completion of the dropwise addition of the alkaline solution; the washing is preferably water washing, and in a specific embodiment of the present invention, the aluminum hydroxide gel is preferably washed with water and centrifuged until the supernatant is neutral; the drying temperature is preferably 50 to 150°C, and the drying time is preferably 6 to 24 hours; the first calcination temperature is preferably 200 to 500°C, preferably 300 to 400°C, the first calcination time is preferably 2 to 10 hours, more preferably 3 to 5 hours, and the heating rate to the first calcination temperature is preferably 2 to 10°C / min; the first calcination is preferably carried out in an air atmosphere.
[0036] After obtaining the alumina carrier, the present invention mixes the alumina carrier, copper salt, water and a reducing agent for reduction deposition, and the obtained reduction deposition product is sequentially roasted (recorded as the second roasting) and reduced to obtain an alumina-supported copper precursor. In the present invention, the copper salt preferably includes one or more of copper chloride, nitrate, sulfate and acetate, more preferably copper nitrate, copper chloride or copper acetate; the copper loading in the alumina-supported copper precursor is preferably 0.1-10wt%, more preferably 3-6wt%, and the copper loading is measured as the percentage of the mass of the copper element to the total mass of the alumina-supported copper precursor; the copper salt is preferably used in the form of a copper salt aqueous solution, and the concentration of the copper salt aqueous solution is preferably 0.005-0.02mol / L.
[0037] In the present invention, the reducing agent is preferably one or more of sodium borohydride, sodium hydride, lithium aluminum tetrahydride, hydrazine hydrate, phenylsilane, formaldehyde, citric acid, sodium citrate and vitamin C, more preferably sodium borohydride, the molar ratio of the reducing agent to the copper salt is preferably 1: (1-10), more preferably 1: (1-5); the temperature of the reduction deposition is preferably 20-80°C, more preferably 25-60°C; the reduction deposition method comprises: first mixing the alumina carrier, copper salt and water, then adding the reducing agent, 0-30 min after adding the reducing agent (0 min, i.e., adding the alkaline solution immediately after the reducing agent is added), adjusting the pH value of the reaction solution to 11-14 using the alkaline solution, and then depositing at 20-80°C for 2-8h.
[0038] In the present invention, the mixing method of the alumina carrier, copper salt and water is preferably to directly add the alumina carrier and copper salt into water for mixing, or preferably to prepare an alumina carrier suspension with alumina carrier and water, prepare copper salt and water into a copper salt aqueous solution, and then add the copper salt solution into the alumina carrier suspension; the alkali in the alkaline solution is preferably at least one of potassium hydroxide, sodium hydroxide, potassium carbonate, potassium bicarbonate, sodium carbonate, sodium bicarbonate and ammonia water; the concentration of the alkaline solution is preferably 0.1-5 mol / L, more preferably 0.2-4 mol / L. In the present invention, after adding the reducing agent, a part of the divalent copper in the solution is reduced to metallic copper and loaded on the alumina, a part of the divalent copper is reduced to monovalent copper, and a part is not reduced. The pH adjusting agent is added at this time in the present invention, which can be used as a precipitant to precipitate divalent and monovalent copper ions onto the carrier. This part of the precipitate will be converted into oxides during the later roasting process and converted into metallic copper during the subsequent H2 reduction process. Through experimental comparison and characterization, it is found that the state and dispersion of the metallic copper obtained by direct reduction in the solution and the metallic copper reduced by roasting are very different. Therefore, the present invention can adjust the type of precipitate and the precipitation speed by adjusting the pH, and can also affect the size, crystal form and dispersion of the copper particles, which is conducive to forming the metallic copper state (including particle size and crystal form and appropriate dispersion) required for the later molecular imprinting experiment.
[0039] After the reduction precipitation is completed, the present invention preferably centrifuges the obtained product liquid until the supernatant is neutral, then removes the supernatant, dries the obtained solid product, and then performs subsequent roasting and reduction on the dried solid product; the detergent used for centrifugal washing is preferably deionized water; the drying temperature is preferably 50 to 150°C, and the drying time is preferably 6 to 24 hours.
[0040] In the present invention, the temperature of the second calcination is preferably 200-500°C, preferably 300-400°C, the time of the second calcination is preferably 2-10h, more preferably 3-5h, and the heating rate to the temperature of the second calcination is preferably 2-10°C / min; the second calcination is preferably carried out in an air atmosphere.
[0041] In the present invention, the reduction is preferably carried out in a reducing gas, the volume fraction of hydrogen in the reducing gas is preferably 5 to 100%, when the volume fraction of hydrogen is less than 100%, the remainder is preferably argon; the flow rate of the reducing gas is preferably 5 to 20 mL / min, more preferably 10 to 15 mL / min; the temperature of the reduction is preferably 250 to 450°C, more preferably 350 to 400°C, the time of the reduction is preferably 2 to 6 hours, more preferably 3 to 5 hours, and the heating rate to the temperature of the reduction is 2 to 10°C / min. After the reduction is completed, the temperature is naturally cooled to room temperature.
[0042] After obtaining an alumina-supported copper precursor, the present invention sequentially adsorbs a template molecule and an organic ligand into the alumina-supported copper precursor by a programmed temperature adsorption method to obtain an alumina-supported copper heterogeneous catalyst having a molecular imprinting function; the template molecule is a nitro compound. The present invention first adsorbs the template molecule and then adsorbs the organic ligand, the template molecule plays the role of a placeholder group in the alumina-supported copper precursor, and the subsequently adsorbed organic ligand is adsorbed around the template molecule to form a cavity with a certain size and shape, thereby ensuring that the obtained catalyst has a molecular imprinting effect.
[0043] In the present invention, the template molecule is preferably one of nitrobenzene and its derivatives, nitronaphthalene and its derivatives, nitropyrene and its derivatives; the structure of the template molecule is preferably a structure shown in any one of Formulas 1 to 3:
[0044]
[0045] In formulas 1 to 3: R 1 , R 2 and R 3 are independently hydrogen, -(C1-C 12 )-alkyl, -(C3-C 12 )-cycloalkyl, -(C3-C 12 )-heterocycloalkyl, (C6-C 20 )-aryl, (C3-C 20 )-heteroaryl, -O-(C1-C 12 )-alkyl, -O-(C3-C 12)-cycloalkyl, phenoxy, halogen, trifluoromethyl, hydroxyl, amino or nitro; in Formula 1: n is preferably 1 to 5, more preferably 1 to 3, and n R 1 The groups are the same or different; in Formula 2: n is 1 to 7, preferably 1 to 3, and n R 2 The groups are the same or different; in Formula 3: n is 1 to 9, preferably 1 to 3, and n R 3 In the present invention, the -(C1-C 12 )-alkyl is preferably -(C1-C6)-alkyl, more preferably methyl, ethyl or propyl; the -(C3-C 12 )-cycloalkyl is preferably cyclopentylcyclohexyl; the -(C3-C 12 )-heterocycloalkyl is preferably piperidinyl; the (C6-C 20 )-aryl is preferably phenyl or methylphenyl; the (C3-C 20 )-heteroaryl is preferably pyridyl or pyrrolyl; the -O-(C1-C 12 )-alkyl is preferably methoxy or ethoxy; the -O-(C3-C 12 )-Cycloalkyl is preferably cyclohexyloxy; the halogen is preferably -Cl, -F or -Br.
[0046] In a specific embodiment of the present invention, the template molecule is preferably nitrobenzene, nitronaphthalene, nitropyrene, 2-methylnitrobenzene, 4-methylnitrobenzene, 4-methoxynitrobenzene, 4-fluoronitrobenzene, 4-chloronitrobenzene, 2,6-dimethylnitrobenzene, 2-methylnitronaphthalene or 1-bromo-5-nitronaphthalene.
[0047] In the present invention, the structure of the organic ligand is preferably a structure shown in any one of Formulas 4 to 12:
[0048]
[0049] In formula 4 to formula 12: R 4 , R 5 , R 6 and R 7 is hydrogen, -(C1-C 12 )-alkyl, -O-(C1-C 12 )-alkyl, halogen, trifluoromethyl, hydroxyl or amine; in Formula 4: n is 1 to 5, preferably 1 to 3, and n R 1 The groups are the same or different; in Formula 5, Formula 7, Formula 8, Formula 10 and Formula 11, n is independently 1 to 4, preferably 1 to 2, m is independently 1 to 4, preferably 1 to 2, and n R 5 The groups are the same or different, m R 6The groups are the same or different; in Formula 6, Formula 9 and Formula 12, n is independently 1 to 8, preferably 1 to 3, and n R 7 In the present invention, the -(C1-C 12 )-alkyl is preferably methyl or ethyl; the -O-(C1-C 12 )-alkyl is preferably methoxy; the halogen is preferably -Cl, -F or -Br.
[0050] In a specific embodiment of the present invention, the organic ligand is preferably 1,10-phenanthroline; the organic ligand is adsorbed on the copper surface to form a molecular imprinting cavity, providing a molecular imprinting function (i.e., high selectivity) for the catalyst. In addition, the organic ligand can also form a Cu-N bond with the copper atom, serving as a new active site for hydrogenation of nitro compounds, thereby improving the hydrogenation activity of the catalyst.
[0051] In the present invention, the method of sequentially adsorbing the template molecule and the organic ligand into the alumina-loaded copper precursor by means of programmed temperature adsorption preferably comprises: placing the template molecule in the middle and upper reaches of a tube furnace, placing the alumina-loaded copper precursor in the middle and lower reaches of the tube furnace, performing a first temperature increase adsorption, and then placing the organic ligand in the middle and upper reaches of the tube furnace, and placing the alumina-loaded copper precursor in the middle and lower reaches of the tube furnace for a second temperature increase adsorption; the present invention preferably places the template molecule (or organic ligand) in a ceramic ark, and then places the ceramic ark containing the template molecule (or organic ligand) in the middle and upper reaches of the tube furnace, placing the alumina-loaded copper precursor in the ceramic ark, and then placing the organic ligand in the middle and upper reaches of the tube furnace, and placing the alumina-loaded copper precursor in the ceramic ark, and then placing the organic ligand in the middle and upper reaches of the tube furnace. The ceramic ark containing the aluminum-loaded copper precursor is placed in the middle and downstream of the tube furnace, and the ceramic ark containing the alumina-loaded copper precursor is preferably placed close to the upstream ark containing the template molecule (or organic ligand); in the present invention, the mass ratio of the template molecule to the alumina-loaded copper precursor is preferably 1-200:5-50, and the mass ratio of the organic ligand to the alumina-loaded copper precursor is preferably 1-100:5-50; in a specific embodiment of the present invention, the loading amount of the template molecule is preferably 10-2000 mg, the loading amount of the organic ligand is preferably 10-1000 mg, and the loading amount of the alumina-loaded copper precursor is preferably 50-500 mg. In the present invention, the temperature of the first temperature rise adsorption is preferably 50-300°C, more preferably 100-200°C, the holding time of the first temperature rise adsorption is preferably 0.5-5h, more preferably 1.5-3h, and the heating rate to the temperature of the first temperature rise adsorption is preferably 0.5-10°C / min, more preferably 1-3°C / min; after the first temperature rise adsorption is completed, it is preferably cooled naturally, and then the ceramic ark with the alumina-loaded copper precursor is kept stationary, and the ceramic ark originally loaded with the template molecule is replaced with the ceramic ark loaded with the organic ligand; the temperature of the second temperature rise adsorption is preferably 50-250°C, more preferably 100-150°C, the holding time of the second temperature rise adsorption is preferably 0.5-5h, more preferably 1-3h, and the heating rate to the temperature of the second temperature rise adsorption is preferably 0.5-10°C / min, more preferably 2-8°C / min, and after the second temperature rise adsorption is completed, the temperature is naturally cooled. In the present invention, the first temperature rise adsorption and the second temperature rise adsorption are preferably carried out in a protective gas. Before the first temperature rise adsorption and the second temperature rise adsorption, it is preferred to use a protective gas to purge for 10 to 30 minutes to replace the internal gas. The protective gas is preferably a reducing gas. The volume fraction of hydrogen in the reducing gas is preferably 5 to 100%, more preferably 10 to 80%. When the volume fraction of hydrogen is less than 100%, the remainder is preferably argon.The present invention uses template molecules and organic ligands to continuously heat up and adsorb the carrier, and the adsorption temperature is between the melting point and boiling point of the template molecules and the organic ligands. During the heating process, the volatilized template molecules or organic ligands are swept to the downstream by the flow of air flow and the action of carrier gas, and are partially adsorbed on the carrier, thereby obtaining an alumina-supported copper multiphase catalyst with molecular imprinting function. Figure 1 Schematic diagram of the continuous temperature increase adsorption process in the present invention, wherein A represents the template molecule and L represents the ligand.
[0052] After the temperature adsorption is completed, the obtained solid product is preferably washed and dried, and the washing detergent is preferably one of alcohol, dioxane, tetrahydrofuran, ethylene glycol dimethyl ether, ethyl acetate, butyl acetate, benzene, toluene, anisole, xylene, dichloromethane, chloroform and chloroform; the number of washings is preferably 3 times, and the amount of detergent used each time is preferably 1 to 2 mL; the drying is preferably vacuum drying, the drying temperature is preferably 30 to 150° C., and the time is preferably 1 to 12 hours.
[0053] The present invention also provides an alumina-supported copper heterogeneous catalyst with molecular imprinting function prepared by the preparation method described in the above scheme, comprising an alumina carrier, copper supported on the alumina carrier, and template molecules and organic ligands adsorbed on the alumina carrier; the mass fraction of copper in the alumina-supported copper heterogeneous catalyst with molecular imprinting function is preferably 4-5%, the mass fraction of the template molecule is preferably 4-7%, and the mass fraction of the organic ligand is preferably 3-5%.
[0054] The present invention also provides the use of the alumina-supported copper heterogeneous catalyst with molecular imprinting function described in the above scheme in catalyzing the hydrogenation reaction of nitro compounds; in the present invention, the nitro compound preferably includes one or more of nitrobenzene and its derivatives, nitronaphthalene and its derivatives, and nitropyrene and its derivatives; specifically, the structure of the nitro compound is preferably a structure shown in any one of Formulas 1 to 3 (see above for the specific structural formula), wherein the type of substituents and the range of values of n are not repeated here; the present invention reduces the nitro group in the nitro compound to an amino group through a hydrogenation reaction to obtain an amino compound.
[0055] In the present invention, the conditions for the hydrogenation reaction preferably include: a hydrogen pressure of 0.5 to 2.5 MPa, preferably 1.5 MPa, a reaction temperature of 100 to 150° C., preferably 120° C., and a reaction time of 8 to 16 h, preferably 12 h.
[0056] In the present invention, the alumina-supported copper heterogeneous catalyst with molecular imprinting function is easy to separate from reactants and products and can be reused. Specifically, after the hydrogenation reaction is completed, the reactants are taken out by centrifugation, and the remaining catalyst can be directly reused after washing. The washing detergent is preferably one of alcohol, dioxane, tetrahydrofuran, ethylene glycol dimethyl ether, ethyl acetate, butyl acetate, benzene, toluene, anisole, xylene, dichloromethane, chloroform and chloroform; the number of washings is preferably 3 times.
[0057] The alumina-supported copper heterogeneous catalyst with molecular imprinting function provided by the present invention has high reaction activity and selectivity for nitro compounds with the same structure as the template molecule, has no activity for other types of nitro compounds, and has a molecular imprinting effect. In a specific embodiment of the present invention, it is preferred to select a catalyst adsorbed with the corresponding template molecule according to the type of nitro compound in the hydrogenation reaction.
[0058] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0059] Example 1
[0060] Weigh 4.28g (11.4mmol) Al(NO3)3·9H2O and dissolve it in 100mL deionized water, then add 30mL of aqueous solution containing 2.71g (25.6mmol) Na2CO3, and continue stirring at 25°C for 5h to obtain a colloid; wash the obtained colloid with water and centrifuge until the supernatant is neutral, and dry it in an oven at 100°C for 12h; grind the dried white solid, and place it in a muffle furnace at 350°C for air roasting for 5h to obtain 560mg white Al2O3 solid.
[0061] 0.15 g (0.6 mmol) Cu(NO3)2·3H2O and 0.6 g of the obtained Al2O3 material were weighed into 100 mL of deionized water, and 10 mL of an aqueous solution containing 0.023 g (0.6 mmol) NaBH4 was added. After stirring for 10 min, 20 mL of an aqueous solution containing 0.076 g (0.72 mmol) Na2CO3 was added to adjust the pH value to 13, and the mixture was stirred at 25°C for 5 h to obtain a reduction deposition product solution; the solid in the product solution was centrifuged and washed with deionized water until the supernatant was neutral; the solid obtained after washing and centrifugation was placed in a common oven at 25°C and dried for 12 h; the dried white solid was ground and then placed in a muffle furnace at 350°C for air roasting for 3 h; the roasted white solid was reduced in a conventional reduction furnace at 350°C for 3 h using a hydrogen atmosphere with a hydrogen flow rate of 10 mL / min, and 600 mg of black alumina-loaded copper precursor was obtained after natural cooling, recorded as Cu / Al2O3.
[0062] Example 2
[0063] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0064] 1230 mg of nitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark loaded with 200 mg of 1,10-phenanthroline was used to replace the ark originally containing the template molecule. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A1-L1.
[0065] Example 3
[0066] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0067] 142 mg of nitronaphthalene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark loaded with 200 mg of 1,10-phenanthroline was used to replace the ark originally containing the template molecule. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A2-L1.
[0068] Example 4
[0069] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0070] 254 mg of nitropyrene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark originally containing the template molecule was replaced with an ark loaded with 200 mg of 1,10-phenanthroline. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A3-L1.
[0071] Example 5
[0072] The catalysts prepared in Examples 1 to 4 were used in the hydrogenation reaction of nitro compounds to illustrate the catalytic performance and molecular imprinting effect of different catalysts in catalyzing reactions of different types of nitro compounds.
[0073] In a 100mL reactor, add 80mg of the above-prepared catalyst, 1mmol of nitro compound and 3mL of toluene, seal and replace the air in the system with pure hydrogen three times, and fill with hydrogen at a total pressure of 1.5MPa. Then heat to 120°C and react for 12h. After stopping the reaction and cooling to room temperature, the reaction solution is analyzed by HP-7890N gas chromatography equipped with an HP-5 capillary column and FID detector, using biphenyl as the internal standard. The reaction data of different catalysts and different types of nitro compounds are shown in Table 1.
[0074] Table 1 Results of the catalysts synthesized in Examples 1 to 4 in catalyzing the hydrogenation of nitro compounds
[0075]
[0076] As can be seen from Table 1, the alumina-supported copper heterogeneous catalyst with molecular imprinting function provided by the present invention is applied to the hydrogenation reaction of different types of nitro compounds, and exhibits high reaction activity and selectivity for nitro compounds with the same molecular structure as the template, but has no activity for other types of nitro compounds, which also shows that the catalyst has a molecular imprinting effect.
[0077] Example 6
[0078] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0079] 1230 mg of nitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark loaded with 79 mg of pyridine was used to replace the ark originally containing the template molecule. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 80°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 60°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A1-L2.
[0080] Example 7
[0081] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0082] 1230 mg of nitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark loaded with 156 mg of 2,2-bipyridine was used to replace the ark originally containing the template molecule. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A1-L3.
[0083] Example 8
[0084] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0085] 1230 mg of nitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark loaded with 200 mg of 1,7-phenanthroline was used to replace the ark originally containing the template molecule. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A1-L4.
[0086] Example 9
[0087] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0088] 1230 mg of nitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark loaded with 200 mg of 4,7-phenanthroline was used to replace the ark originally containing the template molecule. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A1-L5.
[0089] Example 10
[0090] The catalysts prepared in Examples 6 to 10 were used in the hydrogenation reaction of nitro compounds to illustrate the catalytic performance and molecular imprinting effect of different catalysts in catalyzing reactions of different types of nitro compounds.
[0091] In a 100mL reactor, 80mg of the above-prepared catalyst, 1mmol of nitro compound and 3mL of toluene were added. After sealing, the air in the system was replaced with pure hydrogen three times, and hydrogen with a total pressure of 1.5MPa was filled. Then the temperature was raised to 120°C and the reaction was carried out for 12h. After stopping the reaction and cooling to room temperature, the reaction solution was analyzed by HP-7890N gas chromatography equipped with an HP-5 capillary column and an FID detector, using biphenyl as the internal standard. The reaction data of different catalysts and different types of nitro compounds are shown in Table 2.
[0092] Table 2 Results of the catalysts synthesized in Examples 6 to 9 in catalyzing the hydrogenation of nitro compounds
[0093]
[0094] It can be seen from the data in Table 2 that the alumina-supported copper heterogeneous catalyst with molecular imprinting function provided by the present invention is applied to the hydrogenation reaction of different types of nitro compounds, and exhibits high reaction activity and selectivity for nitro compounds with the same molecular structure as the template, and low activity for other types of nitro compounds, which also shows that the catalyst has a molecular imprinting effect; in addition, according to the data in Table 2, it can be seen that when different organic ligands are used, the yield and selectivity of aniline also vary, indicating that the type of organic ligand will also affect the activity and selectivity of the catalyst to a certain extent. Combined with the data in Examples 1 to 9, when the organic ligand is 1,10-phenanthroline, the obtained catalyst has the best activity and selectivity.
[0095] Embodiment 11
[0096] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0097] 1370 mg of 2-methylnitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark loaded with 200 mg of 1,10-phenanthroline was used to replace the ark originally containing the template molecule. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A4-L1.
[0098] Example 12
[0099] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0100] 1370 mg of 4-methylnitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark originally containing the template molecule was replaced with an ark loaded with 200 mg of 1,10-phenanthroline. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A5-L1.
[0101] Embodiment 13
[0102] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0103] 1530 mg 4-methoxynitrobenzene was weighed and loaded into a ceramic ark and the ark was placed in the middle upstream of the tube furnace. 200 mg Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark loaded with 200 mg 1,10-phenanthroline was used to replace the ark originally containing the template molecule. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A6-L1.
[0104] Embodiment 14
[0105] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0106] 1410 mg of 4-fluoronitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg of Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark originally containing the template molecule was replaced with an ark loaded with 200 mg of 1,10-phenanthroline. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A7-L1.
[0107] Embodiment 15
[0108] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0109] 1575 mg 4-chloronitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark loaded with 200 mg 1,10-phenanthroline was used to replace the ark originally containing the template molecule. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A8-L1.
[0110] Example 16
[0111] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0112] 1510 mg 2,6-dimethylnitrobenzene was weighed and loaded into a ceramic ark and the ark was placed upstream of the middle of the tube furnace. 200 mg Cu / Al2O3 was weighed and loaded into a ceramic ark and placed in turn close to another ark in the downstream direction of the tube furnace. At room temperature, 10% hydrogen in argon was used as a protective gas. After continuous purging for 30 minutes, the temperature was gradually increased to 150°C at 2°C / min and the template molecule was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the downstream ark containing Cu / Al2O3 was kept stationary, and the ark originally containing the template molecule was replaced with an ark loaded with 200 mg 1,10-phenanthroline. After continuous purging with 10% hydrogen in argon for 30 minutes, the temperature was gradually increased to 130°C at 5°C / min and the organic ligand was kept adsorbed for 2 hours. After the adsorption was completed and the temperature dropped naturally, the solid was washed with toluene 3 times and dried at 100°C for 12 hours to obtain a dark brown solid, which was recorded as catalyst Cu / Al2O3-A9-L1.
[0113] Embodiment 17
[0114] The catalysts prepared in Examples 11 to 16 were used in the hydrogenation reaction of nitro compounds to illustrate the catalytic performance and molecular imprinting effect of different catalysts in catalyzing reactions of different types of nitro compounds.
[0115] In a 100mL reactor, 80mg of the above-prepared catalyst was added, 1mmol of nitro compound and 3mL of toluene were added, and the air in the system was replaced with pure hydrogen three times after sealing, and hydrogen with a total pressure of 1.5MPa was filled in. Then the temperature was raised to 120°C and the reaction was carried out for 12h. After stopping the reaction and cooling to room temperature, the reaction solution was analyzed by HP-7890N gas chromatography equipped with an HP-5 capillary column and an FID detector, using biphenyl as the internal standard. The reaction data of different catalysts and different types of nitro compounds are shown in Table 3.
[0116] Table 3 Results of the catalysts synthesized in Examples 11 to 16 in catalyzing the hydrogenation of nitro compounds
[0117]
[0118]
[0119] As can be seen from Table 3, the alumina-supported copper heterogeneous catalyst with molecular imprinting function provided by the present invention is applied to the hydrogenation reaction of different types of nitro compounds, and exhibits high reaction activity and selectivity for nitro compounds with the same molecular structure as the template, but has no activity for other types of nitro compounds, which also shows that the catalyst has a molecular imprinting effect.
[0120] Embodiment 18
[0121] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0122] Weigh 150 mg of 2-methylnitronaphthalene into a ceramic ark and place the ark upstream of the middle of the tube furnace; weigh 200 mg of Cu / Al2O3 into a ceramic ark and place it in turn next to another ark in the downstream direction of the tube furnace; use 10% hydrogen in argon as a protective gas at room temperature, purge continuously for 30 minutes, gradually increase the temperature to 150°C at 2°C / min, and keep the template molecule adsorbed for 2 hours; after the adsorption is completed and the temperature drops naturally, keep the downstream ark containing Cu / Al2O3 stationary, replace the ark originally containing the template molecule with an ark loaded with 200 mg of 1,10-phenanthroline, purge continuously for 30 minutes with 10% hydrogen in argon protective gas, gradually increase the temperature to 130°C at 5°C / min, and keep the organic ligand adsorbed for 2 hours; after the adsorption is completed and the temperature drops naturally, wash the solid with toluene 3 times, dry it at 100°C for 12 hours, and finally obtain a dark brown solid, which is recorded as catalyst Cu / Al2O3-A 10 -L1.
[0123] Embodiment 19
[0124] The preparation method of the alumina-supported copper precursor is the same as that in Example 1.
[0125] Weigh 202 mg of 1-bromo-5-nitronaphthalene into a ceramic ark and place the ark in the middle upstream of the tube furnace, weigh 200 mg of Cu / Al2O3 into a ceramic ark and place it in turn next to another ark in the downstream direction of the tube furnace; use 10% hydrogen in argon as a protective gas at room temperature, purge continuously for 30 minutes, gradually heat up to 150°C at 2°C / min, and keep the template molecule adsorbed for 2 hours; after the adsorption is completed and the temperature drops naturally, keep the downstream ark containing Cu / Al2O3 stationary, replace the ark originally containing the template molecule with an ark loaded with 200 mg of 1,10-phenanthroline, purge continuously for 30 minutes with 10% hydrogen in argon protective gas, gradually heat up to 130°C at 5°C / min, and keep the organic ligand adsorbed for 2 hours; after the adsorption is completed and the temperature drops naturally, wash the solid with toluene 3 times, dry it at 100°C for 12 hours, and finally obtain a dark brown solid, which is recorded as catalyst Cu / Al2O3-A 11 -L1.
[0126] Embodiment 20
[0127] The catalysts prepared in Examples 18 to 19 were used in the hydrogenation reaction of nitro compounds to illustrate the catalytic performance and molecular imprinting effect of different catalysts in catalyzing reactions of different types of nitro compounds.
[0128] In a 100mL reactor, 80mg of the above-prepared catalyst, 1mmol of nitro compound and 3mL of toluene were added. After sealing, the air in the system was replaced with pure hydrogen three times, and hydrogen with a total pressure of 1.5MPa was filled. Then the temperature was raised to 120°C and the reaction was carried out for 12h. After stopping the reaction and cooling to room temperature, the reaction solution was analyzed by HP-7890N gas chromatography equipped with an HP-5 capillary column and an FID detector, using biphenyl as the internal standard. The reaction data of different catalysts and different types of nitro compounds are shown in Table 4.
[0129] Table 4 Results of the catalysts synthesized in Examples 13 to 14 in catalyzing the hydrogenation of nitro compounds
[0130]
[0131] As can be seen from Table 4, the alumina-supported copper heterogeneous catalyst with molecular imprinting function provided by the present invention is applied to the hydrogenation reaction of different types of nitro compounds, and exhibits high reaction activity and selectivity for nitro compounds with the same molecular structure as the template, but has no activity for other types of nitro compounds, which also shows that the catalyst has a molecular imprinting effect.
[0132] Embodiment 21
[0133] Taking the catalyst Cu / Al2O3-A1-L1 as an example, the performance of the alumina-supported copper heterogeneous catalyst with molecular imprinting function in the catalytic hydrogenation reaction of nitro compounds is demonstrated.
[0134] Reaction conditions: 80 mg of catalyst Cu / Al2O3-A1-L1 and 123 mg (1 mmol) of nitrobenzene were placed in a 100 mL autoclave, and 3 mL of toluene was added. The gas in the autoclave was replaced with hydrogen, and the process was repeated three times. The hydrogen pressure was 1.5 MPa, and the reaction was carried out at 120°C for 12 hours. After the reaction, the reactants were centrifuged and taken out. The catalyst was washed three times with 2 mL of toluene and then directly placed in the autoclave for reuse. The reaction solution was analyzed using an HP-7890N gas chromatograph equipped with an HP-5 capillary column and an FID detector, with biphenyl as the internal standard. The reaction data of the catalyst reuse are shown in Table 5:
[0135] Table 5 Performance of catalysts for repeated use in catalytic hydrogenation of nitro compounds
[0136]
[0137] It can be seen from Table 5 that the catalyst prepared by the present invention can be reused, and during repeated use, it still has the same catalytic activity and molecular imprinting effect as when it was initially used.
[0138] Test Case
[0139] The Cu / Al2O3 prepared in Example 1 and the Cu / Al2O3-A1-L1 prepared in Example 2 were characterized and tested after being used once; at the same time, according to the method of Example 2, the adsorption process of the organic ligand was omitted to obtain Cu / Al2O3-A1; according to the method of Example 2, the adsorption process of the template molecule was omitted to obtain Cu / Al2O3-L1; Cu / Al2O3-A1 and Cu / Al2O3-L1 were characterized and tested.
[0140] Test results such as Figure 2 As shown, Figure 2 Middle: (a) TGA graph, (b) infrared diffuse reflectance spectrum; in (a) to (b): i represents Cu / Al2O3, ii represents Cu / Al2O3-A1, iii represents Cu / Al2O3-L1, iv represents Cu / Al2O3-A1-L1, and v represents Cu / Al2O3-A1-L1 after use.
[0141] according to Figure 2From the test results in (a), we can see that compared with Cu / Al2O3 (curve i), Cu / Al2O3-A1 (curve ii) and Cu / Al2O3-L1-A1 (curve iii) both have a certain degree of weight loss, which is mainly due to the adsorption of (nitrobenzene) and L1 (1,10-phenanthroline) on the copper precursor supported by alumina. Figure 2 (b) Nitro group (curve ii, 1530 cm -1 and 1350cm -1 Nearby, from nitrobenzene) and C=N (curve iii, 1380 cm -1 The results are consistent with those in the infrared characteristic peaks of 1,10-phenanthroline. Figure 2 The results in (a) show that Cu / Al2O3-A1-L1 (curve iv) also loses weight, and the weight loss rate is higher than that of Cu / Al2O3-A1 (curve ii), indicating that after adsorbing nitrobenzene in the first temperature-raising adsorption process, 1,10-phenanthroline is also successfully adsorbed in the second temperature-raising adsorption stage, and the catalyst with molecular imprinting function described in the article is successfully prepared. Due to the adsorption of nitrobenzene as a template molecule in the early stage, it occupies a certain spatial position on the surface of the copper precursor, resulting in a decrease in the adsorption amount of the ligand. In terms of thermogravimetry, the weight loss rate of Cu / Al2O3-A1-L1 (curve iv) is lower than that of Cu / Al2O3-L1 (curve iii). The weight loss rate of Cu / Al2O3-A1-L1 (curve v) after reaction is lower than that of Cu / Al2O3-A1-L1 (curve iv) before use, indicating that there is molecular desorption or loss on the catalyst surface. According to the results of infrared diffuse reflectance ( Figure 2 As can be seen from (b), the characteristic peak of nitro group still exists in Cu / Al2O3-A1-L1 (curve iv) before use, and the characteristic peak of nitro group disappears in Cu / Al2O3-A1-L1 (curve v) after use, while the characteristic peak of C=N still exists, indicating that the ligand on the surface of copper precursor can exist stably. It also shows that the difference in weight loss rate in thermogravimetric analysis mainly comes from the conversion or desorption of template molecule nitrobenzene in the subsequent hydrogenation reaction.
[0142] Based on the above results, it can be seen that after two stages of temperature increase adsorption, nitrobenzene and 1,10-phenanthroline were successfully adsorbed on the surface of the copper precursor, and an alumina-supported copper heterogeneous catalyst with molecular imprinting function was prepared. The catalyst has a certain stability after the hydrogenation reaction of nitro compounds.
[0143] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an alumina-supported copper heterogeneous catalyst having molecular imprinting function, characterized in that: The following steps are involved: The aluminum oxide carrier, copper salt, water and reducing agent are mixed for reduction deposition, and the obtained reduction deposition product is sequentially calcined and reduced to obtain an aluminum oxide-supported copper precursor; The template molecule and the organic ligand are sequentially adsorbed into the alumina-supported copper precursor by a programmed temperature adsorption method to obtain an alumina-supported copper heterogeneous catalyst with molecular imprinting function; the template molecule is a nitro compound; the organic ligand is one of pyridine and its derivatives, bipyridine and its derivatives, or phenanthroline and its derivatives.
2. The preparation method according to claim 1, characterized in that: The preparation method of the alumina carrier comprises: mixing an aluminum salt solution and an alkaline solution to perform a precipitation reaction to obtain an aluminum hydroxide gel; and sequentially washing, drying and calcining the aluminum hydroxide gel to obtain the alumina carrier.
3. The preparation method according to claim 1, characterized in that: The copper salt includes one or more of copper chloride, nitrate, sulfate and acetate; the copper loading in the alumina-loaded copper precursor is 0.1-10 wt%; The reducing agent is one or more of sodium borohydride, sodium hydride, lithium aluminum tetrahydride, hydrazine hydrate, phenylsilane, formaldehyde and vitamin C; the molar ratio of the reducing agent to the copper salt is 1:(1-10); the temperature of the reduction deposition is 20-80°C; The reduction deposition method comprises: firstly mixing the alumina carrier, copper salt and water, then adding a reducing agent, adjusting the pH value of the reaction solution to 11-14 using an alkaline solution 0-30 minutes after adding the reducing agent, and then depositing at 20-80°C for 2-8 hours.
4. The preparation method according to claim 1, characterized in that: The calcination temperature is 200-500°C, the time is 2-10h, and the heating rate to the calcination temperature is 2-10°C / min; The reduction is carried out in a reducing gas, the volume fraction of hydrogen in the reducing gas is 5 to 100%; the flow rate of the reducing gas is 5 to 20 mL / min; the reduction temperature is 250 to 450° C., the reduction time is 2 to 6 hours, and the heating rate to the reduction temperature is 2 to 10° C. / min.
5. The preparation method according to claim 1, characterized in that: The method for sequentially adsorbing template molecules and organic ligands into the alumina-loaded copper precursor by means of programmed temperature adsorption comprises: placing the template molecules in the middle and upper reaches of a tubular furnace, placing the alumina-loaded copper precursor in the middle and lower reaches of the tubular furnace, performing a first temperature-raising adsorption, then placing the organic ligands in the middle and upper reaches of the tubular furnace, and placing the alumina-loaded copper precursor adsorbed with the template molecules in the middle and lower reaches of the tubular furnace for a second temperature-raising adsorption; the temperature of the first temperature-raising adsorption is 50 to 300°C, the insulation time is 0.5 to 5h, and the heating rate from heating to the temperature of the first temperature-raising adsorption is 0.5 to 10°C / min; the temperature of the second temperature-raising adsorption is 50 to 250°C, the insulation time is 0.5 to 5h, and the heating rate from heating to the temperature of the second temperature-raising adsorption is 0.5 to 10°C / min.
6. The preparation method according to claim 1, characterized in that: The template molecule is one of nitrobenzene and its derivatives, nitronaphthalene and its derivatives, nitropyrene and its derivatives.
7. The preparation method according to claim 1 or 6, characterized in that: The structure of the template molecule is any one of Formulas 1 to 3: In formulas 1 to 3: R 1 , R 2 and R 3 are independently hydrogen, -(C1-C 12 )-alkyl, -(C3-C 12 )-cycloalkyl, -(C3-C 12 )-heterocycloalkyl, (C6-C 20 )-aryl, -O-(C1-C 12 )-alkyl, -O-(C3-C 12 )-cycloalkyl, phenoxy, halogen, trifluoromethyl, hydroxyl, amino or nitro; wherein n is 1 to 5, and n R 1 The groups are the same or different; in formula 2: n is 1 to 7, and n R 2 The groups are the same or different; in formula 3: n is 1 to 9, and n R 3 The groups are the same or different; The structure of the organic ligand is any one of formulas 4 to 12: In formula 4 to formula 12: R 4 , R 5 , R 6 and R 7 is hydrogen, -(C1-C 12 )-alkyl, -O-(C1-C 12 )-alkyl, halogen, trifluoromethyl, hydroxyl or amine; in Formula 4: n is 1 to 5, and n R 4 The groups are the same or different; in Formula 5, Formula 7, Formula 8, Formula 10 and Formula 11, n is independently 1 to 4, m is independently 1 to 4, and n R 5 The groups are the same or different, m R 6 The groups are the same or different; in Formula 6, Formula 9 and Formula 12, n is independently 1 to 8, and n R 7 The groups may be the same or different.
8. Alumina-supported copper heterogeneous catalyst with molecular imprinting function prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The invention comprises an alumina support, copper loaded on the alumina support, and template molecules and organic ligands adsorbed on the alumina support.
9. Use of the alumina-supported copper heterogeneous catalyst with molecular imprinting function as claimed in claim 8 in catalyzing the hydrogenation reaction of nitro compounds.
10. The use according to claim 9, characterized in that: The nitro compound includes one of nitrobenzene and its derivatives, nitronaphthalene and its derivatives, and nitropyrene and its derivatives.
Citation Information
Patent Citations
Method for rapid, high-efficiency and selective degradation of trace benzopyrene in water
CN104108783A
Supported non-noble metal catalyst and preparation and application thereof
CN105749948A