A quaternary ammonium silane-modified nano calcium hydroxide hybrid material and preparation and use method thereof
The nano-calcium hydroxide-quaternary ammonium silane hybrid material prepared by the liquid phase precipitation method combines the reinforcement effect of nano-calcium hydroxide and the antibacterial properties of quaternary ammonium silane to solve the existing technology problems in the anti-fungal and anti-bacterial functions of nano-calcium hydroxide in cultural relics. In order to solve the problem of poor protection effect, it has achieved the improvement of mechanical strength and mold suppression of stone cultural relics, and has high commercialization potential.
Patent Information
- Application Number
- CN202310210055.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-26
AI Technical Summary
Existing nano-calcium hydroxide materials are not very effective in protecting cultural relics against mold and bacteria. Their preparation is complex and costly, making it difficult to produce on a large scale and unable to effectively inhibit mold growth.
Nano-calcium hydroxide is prepared using a liquid phase precipitation method, and then quaternary ammonium silane and nano-calcium hydroxide are mixed in a ratio of 1:10 to 1:3 to prepare a nano-calcium hydroxide-quaternary ammonium silane hybrid material. Stone cultural relics are treated to significantly improve their mechanical strength and inhibit mold growth.
This material is simple and low-cost. It can prepare 100 to 120 liters at a time. It can effectively improve the mechanical strength of stone cultural relics and inhibit the growth of mold within 3 to 5 months. It solves the problem of nano-calcium hydroxide material being reinforced alone but without prevention. The problem of mildew protection has commercial prospects.
Smart Images

Figure CN116216758B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the research field of cultural relics protection materials and relates to a quaternary ammonium silane-modified nano calcium hydroxide hybrid material and a preparation and use method thereof. Background Art
[0002] Mold growth is extremely harmful to cultural relics and is an important problem in cultural relic protection. On the one hand, mold hyphae will penetrate and grow in the matrix of cultural relics, causing mechanical damage, and when they grow to a certain amount, they will cover the surface of the cultural relics, seriously affecting the structure and artistic value of the cultural relics; on the other hand, the continuous metabolism of mold during growth will produce pigments and acidic substances, which will pollute the cultural relics and continuously erode the material of the cultural relics (Chem 2021,7,629-669.Nature Microbiology2017,2,16275). At present, the anti-mold and antibacterial protection of cultural relics (ancient murals, stone cultural relics, etc.) has become one of the important research directions of cultural relic protection. With the continuous advancement of nanomaterials and technologies, nanomaterials have been applied in many fields with their unique advantages. At present, the development of nanomaterials in the mildew and antibacterial properties of cultural relics is in full swing. The reported nanomaterials for mildew and antibacterial properties of cultural relics include nanosilver, nanotitanium dioxide, nanozinc oxide, etc. (Nanomaterials 2020, 10, 335. Environmental Science and Pollution Research 2014, 21, 13278-13286). However, the preparation of the above materials is complex, the cost is high, and it is difficult to produce on a large scale.
[0003] Nano calcium hydroxide is a promising inorganic nanomaterial in the protection of cultural relics such as murals, stone and paper. Around 2000, Italian scholar Piero Baglioni and his research team prepared nano calcium hydroxide and applied it to the restoration of church murals, achieving good results, and nano calcium hydroxide is highly compatible with murals, has no negative impact on cultural relics, and can ensure high safety (Langmuir 2001,17,4251-4255). Subsequently, nano calcium hydroxide was successfully applied to the deacidification protection of paper and wooden cultural relics (Langmuir 2005,21,10743-10748). In recent years, nano calcium hydroxide has also achieved good results in the reinforcement of stone cultural relics, lime mortar and earthen sites (Construction and Building Materials 2020,230,117112.Journal of Colloid and Interface Science2019,539,504-515), and has become an ideal inorganic cultural relic reinforcement material.
[0004] The team proposed a new synthesis method for nano calcium hydroxide powder materials (ChemNanoMat 2019, 5, 1152-1158), and synthesized nano calcium hydroxide / hexagonal boron nitride nanocomposites (ACS Applied Materials & Interfaces 2019, 11, 11792-11799) and other materials, which were successfully applied to the reinforcement of murals, and nano calcium hydroxide / nano kaolin nanocomposites (Construction and Building Materials 2021, 300, 124312.) and successfully applied to the reinforcement of sandstone dinosaur fossils, and both have been authorized patents (CN201711361358.7, CN201710491654.2, CN201810526653.1). However, after testing, the above materials only have a reinforcement effect, weak antibacterial effect, and basically do not have an effective mildew protection function in cultural relics protection. Summary of the invention
[0005] Technical issues to be solved
[0006] In order to avoid the shortcomings of the prior art, the present invention proposes a quaternary ammonium silane-modified nano calcium hydroxide hybrid material and a preparation and use method. First, nano calcium hydroxide is prepared by liquid phase precipitation method. Then, quaternary ammonium silane and nano calcium hydroxide are mixed in a ratio of 1:10 to 1:3, and the nano calcium hydroxide-quaternary ammonium silane hybrid material can be obtained after 2 to 5 minutes of reaction. The preparation process of the hybrid material is simple, low-cost, controllable, and has a large output. 100 to 120 liters can be prepared at a single time on a laboratory scale. In practical applications, it is found that the nano calcium hydroxide-quaternary ammonium silane hybrid material can effectively improve the mechanical strength of stone cultural relics. More importantly, after the material is applied to the surface of stone cultural relics, it is found that there is no mold growth for at least 3 to 5 months. The material has great commercial prospects and can be further promoted to the mildew and antibacterial protection of cultural relics such as ancient murals and paper cultural relics.
[0007] Technical Solution
[0008] A quaternary ammonium silane-modified nano-calcium hydroxide hybrid material, characterized in that the mass ratio of quaternary ammonium silane to nano-calcium hydroxide is 1:10-1:3.
[0009] A method for preparing the quaternary ammonium silane-modified nano calcium hydroxide hybrid material, characterized in that the steps are as follows:
[0010] Step 1: Evenly disperse the nano calcium hydroxide powder in deionized water by ultrasonic oscillation, and add NaOH solution to adjust the pH to 8-11;
[0011] Step 2: Add the methanol solution of quaternary ammonium silane dropwise to the solution of step 1 and stir to mix, wherein the mass ratio of quaternary ammonium silane to nano calcium hydroxide is 1:10 to 1:3;
[0012] Step 3: Use methanol to centrifugally wash and dry to obtain powder of nano calcium hydroxide-quaternary ammonium silane hybrid material.
[0013] The nano calcium hydroxide powder is prepared by the method published in Patent No. 201711361358.7.
[0014] In the step 1, 300 to 500 g of nano calcium hydroxide powder is mixed with 110 to 130 liters of deionized water.
[0015] The stirring and mixing in step 2 is for 2 to 5 minutes.
[0016] The methanol solution of quaternary ammonium silane is commercially available.
[0017] An application of the quaternary ammonium silane-modified nano calcium hydroxide hybrid material is characterized in that it is used for mildew-proof protection of stone cultural relics.
[0018] An application method of the quaternary ammonium silane modified nano calcium hydroxide hybrid material is characterized in that 5 grams of quaternary ammonium silane modified nano calcium hydroxide hybrid material powder is added to each liter of ethanol, and the mixture is coated on the surface of stone cultural relics, and mold is not grown for at least 3 to 5 months.
[0019] Beneficial Effects
[0020] The invention proposes a quaternary ammonium silane-modified nano calcium hydroxide hybrid material and a preparation and use method thereof. First, nano calcium hydroxide powder is synthesized, and then quaternary ammonium silane is mixed and stirred with a nano calcium hydroxide dispersion to react quickly to prepare a nano calcium hydroxide-quaternary ammonium silane hybrid material. The material can be prepared at a laboratory scale of 100 to 120 liters at a time. Through applied research, it is found that the nano calcium hydroxide-quaternary ammonium silane hybrid material has a reinforcing effect on stone cultural relics and can effectively improve the mechanical strength of stone cultural relics; in addition, the stone cultural relics treated with the nano calcium hydroxide-quaternary ammonium silane hybrid material have no mold growth for at least 3 to 5 months, while the stone cultural relics treated with pure nano calcium hydroxide have mold growth after 2 days, and do not have anti-mold protection function. The nano calcium hydroxide-quaternary ammonium silane hybrid material has low preparation cost and high yield. The strength of stone cultural relics can be effectively improved by simple treatment, and mold growth can be inhibited for a long time (3 to 5 months), which is conducive to the long-term preservation of stone cultural relics; in contrast, the nano calcium hydroxide material can only reinforce stone cultural relics, and additional anti-mold protection means need to be introduced. This material has excellent social and economic benefits, and is expected to be further promoted to the anti-mildew and antibacterial protection of murals, paper and other cultural relics. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The bactericidal effect of the nano calcium hydroxide-quaternary ammonium silane hybrid material prepared in Example 1 on Aspergillus niger, and the comparison with the unmodified nano calcium hydroxide material
[0022] Figure 2 The anti-mildew effect of the nano calcium hydroxide-quaternary ammonium silane hybrid material prepared in Example 1 on sandstone samples, and the comparison with the unmodified nano calcium hydroxide material DETAILED DESCRIPTION
[0023] The present invention will now be further described with reference to the embodiments and the accompanying drawings:
[0024] The present invention provides a nano calcium hydroxide-quaternary ammonium silane hybrid material and a preparation method thereof, wherein the content of quaternary ammonium silane is adjustable within the range of 10% to 30%, and the preparation is mainly carried out by the following steps:
[0025] Step 1, preparation of nano calcium hydroxide: The preparation of nano calcium hydroxide is based on our previous patent (CN201711361358.7), and the specific steps are as follows: At room temperature, calcium chloride is dissolved in N,N-dimethylformamide and stirred on a magnetic stirrer for 5 minutes. Pour the stirred calcium chloride solution into the prepared sodium hydroxide solution to generate nano calcium hydroxide. The molar ratio of calcium chloride to sodium hydroxide is 1:2. The product is centrifuged, the precipitate is washed 3 times with saturated lime water, and then dried at 60 degrees Celsius for 6 hours to obtain nano calcium hydroxide powder.
[0026] Step 2, preparation of nano calcium hydroxide-quaternary ammonium silane hybrid material: 300-500g of nano calcium hydroxide powder is uniformly dispersed in 110-130 liters of deionized water by ultrasonic oscillation, and NaOH solution is added to adjust the pH to 8-11; a methanol solution of quaternary ammonium silane (commercially available) is taken and added dropwise to the nano calcium hydroxide solution, and the ratio of quaternary ammonium silane to nano calcium hydroxide is 1:10-1:3. The mixed solution is vigorously stirred for 2-5 minutes, and 100-120 liters can be prepared at a time. The powder of nano calcium hydroxide-quaternary ammonium silane hybrid material can be obtained after centrifugal washing with methanol and drying.
[0027] Embodiment 1:
[0028] 500g of prepared nano calcium hydroxide was dispersed uniformly in 130 liters of deionized water by ultrasonic oscillation, NaOH was added to adjust the pH to 8, and then 83g of commercially available quaternary ammonium silane methanol solution (60%) was added dropwise, wherein the ratio of quaternary ammonium silane to nano calcium hydroxide was 1:10. Vigorously stirred for 2 minutes to react, nano calcium hydroxide-quaternary ammonium silane hybrid material can be obtained, 120 liters were prepared at a time, and the precipitate was washed twice with methanol after centrifugation and dried, and finally nano calcium hydroxide-quaternary ammonium silane hybrid material powder was obtained. The yield was about 80%.
[0029] The nano calcium hydroxide-quaternary ammonium silane hybrid material powder was prepared into a 5g / L ethanol dispersion and sprayed on the surface of the simulated sandstone cultural relic sample. After complete penetration, the spraying was repeated for a total of three times. The simulated sandstone cultural relic sample treated with nano calcium hydroxide was used as a comparison.
[0030] Test results: The strength of sandstone treated with nano-calcium hydroxide-quaternary ammonium silane hybrid material and nano-calcium hydroxide increased by 50% and 55% respectively. Through the Aspergillus niger cultivation experiment, it was found that the sandstone samples treated with nano-calcium hydroxide-quaternary ammonium silane hybrid material had no mold growth within 3 months, while the sandstone treated with unmodified nano-calcium hydroxide material had a large amount of mold growth after 2 days.
[0031] Embodiment 2:
[0032] 300g of the prepared nano calcium hydroxide was dispersed uniformly in 110 liters of deionized water by ultrasonic oscillation, NaOH was added to adjust the pH to 11, and then 100g of commercially available quaternary ammonium silane methanol solution (60%) was added dropwise, wherein the ratio of quaternary ammonium silane to nano calcium hydroxide was 1:5. After vigorous stirring for 4 minutes, the nano calcium hydroxide-quaternary ammonium silane hybrid material was obtained, and 100 liters could be prepared at a time. After centrifugation, the precipitate was washed twice with methanol and dried to finally obtain the nano calcium hydroxide-quaternary ammonium silane hybrid material powder. The yield was about 85%.
[0033] The nano calcium hydroxide-quaternary ammonium silane hybrid material powder was prepared into a 5g / L ethanol dispersion and sprayed on the surface of the simulated sandstone cultural relic sample. After complete penetration, the spraying was repeated for a total of three times. The simulated sandstone cultural relic sample treated with nano calcium hydroxide was used as a comparison.
[0034] Test results: The strength of sandstone treated with nano-calcium hydroxide-quaternary ammonium silane hybrid material and nano-calcium hydroxide increased by 51% and 52% respectively. Through the Aspergillus niger cultivation experiment, it was found that the sandstone treated with nano-calcium hydroxide-quaternary ammonium silane hybrid material had no mold growth within 4 months, while the sandstone treated with unmodified nano-calcium hydroxide material had a large amount of mold growth after 2 days.
[0035] Embodiment three:
[0036] 400g of the prepared nano calcium hydroxide was dispersed uniformly in 120 liters of deionized water by ultrasonic oscillation, NaOH was added to adjust the pH to 12, and then 222g of commercially available quaternary ammonium silane methanol solution (60%) was added dropwise, wherein the ratio of quaternary ammonium silane to nano calcium hydroxide was about 1:3. The reaction was vigorously stirred for 5 minutes to obtain a nano calcium hydroxide-quaternary ammonium silane hybrid material, and 105 liters could be prepared at a time. After centrifugation, the precipitate was washed twice with methanol and dried to finally obtain a nano calcium hydroxide-quaternary ammonium silane hybrid material powder.
[0037] The nano calcium hydroxide-quaternary ammonium silane hybrid material powder was prepared into a 5g / L ethanol dispersion and sprayed on the surface of the simulated limestone cultural relic sample. After complete penetration, the spraying was repeated for a total of three times. The simulated limestone cultural relic sample treated with nano calcium hydroxide was used as a comparison.
[0038] Test results: The strength of limestone treated with nano-calcium hydroxide-quaternary ammonium silane hybrid material and nano-calcium hydroxide increased by 52% and 54% respectively. Through the Aspergillus niger cultivation experiment, it was found that the limestone treated with nano-calcium hydroxide-quaternary ammonium silane hybrid material had no mold growth within 5 months, while the limestone treated with unmodified nano-calcium hydroxide material had a large amount of mold growth after 2 days.
[0039] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. An application of a quaternary ammonium silane-modified nano calcium hydroxide hybrid material, characterized in that: Used for anti-mold protection of stone cultural relics; specifically, adding 5 grams of quaternary ammonium silane-modified nano-calcium hydroxide hybrid material powder to each liter of ethanol, mixing and applying it on the surface of stone cultural relics, and no mold will grow for at least 3 months; The quaternary ammonium silane-modified nano calcium hydroxide hybrid material is prepared according to the following steps: Step 1: Evenly disperse the nano calcium hydroxide powder in deionized water by ultrasonic oscillation, and add NaOH solution to adjust the pH to 8-11; Step 2: Add the methanol solution of quaternary ammonium silane dropwise to the solution of step 1 and stir to mix, wherein the mass ratio of quaternary ammonium silane to nano calcium hydroxide is 1:3 or 1:10; Step 3: using methanol to centrifugally wash and dry to obtain powder of nano calcium hydroxide-quaternary ammonium silane hybrid material; In the step 1, 300-500 g of nano calcium hydroxide powder is mixed with 110-130 liters of deionized water; The stirring and mixing in step 2 is 2 to 5 minutes; The prepared nano calcium hydroxide-quaternary ammonium silane hybrid material powder is used for mildew protection of stone cultural relics, specifically comprising: adding 5 grams of quaternary ammonium silane-modified nano calcium hydroxide hybrid material powder into each liter of ethanol, mixing and applying the mixture on the surface of the stone cultural relics, and no mildew will grow for at least 3 months.