A novel continuous cool breathable fabric, preparation method and application thereof

By treating the combination of isocyanate and carboxylic acid group compounds with sodium bisulfite to generate a gel film, combined with the sandwich fabric process, the problem of poor cooling effect of textiles is solved, the preparation of efficient breathable fabrics with continuous coolness is achieved, and the cost of printing and dyeing materials is reduced. Curing control difficulty.

CN116219760BActive Publication Date: 2024-10-18QINGDAO SHANGYA HOUSEWARE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310332452.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-18
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing textiles have poor cooling effects, and the application of polyurethane gel in the textile field is complex and costly, making it difficult to achieve sustained cooling and breathable fabrics.

Method used

Sodium bisulfite compounds are used to block the isocyanate, mixed with compounds containing carboxylic acid groups or polyether polyol compounds, and then unblocked after high-temperature heating to form a continuous cooling gel film, which is combined with the sandwich fabric The process produces breathable fabrics with excellent continuous cooling function.

Benefits of technology

It significantly improves the heat absorption and cooling effect of textiles, reduces the difficulty of curing control of isocyanate printing and dyeing materials, and achieves a significant improvement in the continuous cooling function.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116219760B_ABST
    Figure CN116219760B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of textile printing and dyeing, and in particular to a novel continuous cool breathable fabric, a preparation method and an application thereof. The method uses a sodium bisulfite compound to firstly perform an end-capping treatment on an isocyanate, then mixes and treats the end-capping treatment with a compound containing a carboxylic acid group or a polyether polyol compound before curing, and then unblocks the end-capping treatment after high-temperature heating. The two undergo a curing reaction to generate a continuous cool gel film. The processed continuous cool breathable fabric has an excellent continuous cool function and makes the curing of a printing and dyeing material containing an isocyanate easier to control. The method comprises the following steps: step 1, preparing a continuous cool gel; step 2, preparing a sandwich fabric; step 3, printing, coating and impregnation; step 4, molding; and step 5, packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile printing and dyeing, and in particular to a novel continuous cool breathable fabric, a preparation method and application thereof. Background Art

[0002] The hot weather in summer affects people's work and rest and mood. In order to reduce the impact of hot weather on people, a breathable sports fabric disclosed in the invention patent with the authorization announcement number CN113290960B has been developed. The breathable sports fabric mainly consists of a base fabric layer, an antibacterial and deodorizing layer, and a wear-resistant layer. When used, the breathable sports fabric has the characteristics of wrinkle resistance, antibacterial and wear resistance, but its cooling effect is poor.

[0003] Polyurethane gel has a good continuous cooling effect and is used in products such as sponge bedding, cushions, and backrest cushions. However, during the production process, due to the rapid reaction of multi-component raw materials after mixing, the initial viscosity and solidification time are uncontrollable. It is only suitable for injecting multi-component raw materials into molds for solidification molding, and then attaching them to sponges, cushions, and backrests. The process is complicated and the cost is high. It is difficult to use in the textile field, resulting in poor practicality.

[0004] Therefore, there is an urgent need for a new type of continuously cool breathable fabric, a preparation method and application thereof to improve existing textiles. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a novel continuous cool breathable fabric, preparation method and application thereof, which comprises the steps of first end-capping isocyanate with a sodium bisulfite compound, then mixing and treating the end-capping with a compound containing a carboxylic acid group or a polyether polyol compound before curing, unblocking the end-capping with high-temperature heating, and performing a curing reaction between the two to generate a continuous cool gel film. The processed continuous cool breathable fabric has an excellent continuous cool function and makes the curing of a printing and dyeing material containing isocyanate easier to control.

[0006] A method for preparing a novel continuous cool breathable fabric of the present invention comprises the following steps:

[0007] Step 1: Preparation of continuous cooling gel

[0008] The isocyanate used is blocked with sodium bisulfite, and then the blocked isocyanate is pre-cured with a compound containing a carboxylic acid group or a polyether polyol compound to make the isocyanate resin gel curing process controllable, and then allowed to stand for 60 minutes to degas for use;

[0009] Step 2: Sandwich fabric preparation

[0010] A surface silk layer, a supporting breathable layer and a bottom silk layer are prepared by using a knitting machine, and the surface silk layer is located on the supporting breathable layer, and the supporting breathable layer is located between the surface silk layer and the bottom silk layer to form a sandwich fabric;

[0011] Step 3: Printing, coating and impregnation

[0012] A printing machine is used to perform printing, coating and impregnation processes on the top surface of the sandwich fabric surface silk layer, and the continuous cooling gel is printed on the top surface of the sandwich fabric surface silk layer;

[0013] Step 4: Molding

[0014] Pre-baking is performed at a temperature of 100-140°C for 3-10 minutes, and then baking is performed at a temperature of 130°-160°C for 5-15 minutes to unblock the blocked isocyanate, and the printed and dyed surface containing carboxylic acid compounds or polyether polyol compounds is cured to form a thermosetting continuous cooling gel coating layer of the continuous cooling gel, thereby forming a coated gel sandwich fabric with significant continuous cooling function;

[0015] Step 5: Packaging

[0016] Pack the finished fabrics and store them in warehouse.

[0017] Preferably, in step 2, the surface silk layer is composed of 2 polyester fully stretched filaments FDY with a fineness between 50D-500D, the supporting breathable layer is composed of polyester fully stretched monofilament FDY with a fineness between 24D-300D, and the bottom silk layer is composed of polyester fully stretched filament FDY with a fineness between 50D-500D.

[0018] Preferably, the isocyanate in step 1 can be aliphatic isocyanate, aromatic isocyanate or a mixture of aliphatic isocyanate and aromatic isocyanate in any proportion.

[0019] Preferably, in the step 1, the molar ratio of sodium bisulfite to isocyanate is 1-1.2:1, and the molar ratio of polyether polyol to isocyanate is 100:15-25.

[0020] Preferably, the isocyanate system in step 1 is hydrophilic and soluble in aqueous solution.

[0021] Preferably, in step 4, pre-baking is performed at a temperature of 100-120° C. for 3-6 minutes, and then baking is performed at a temperature of 130°-150° C. for 5-10 minutes.

[0022] The novel continuous cool breathable fabric of the present invention comprises a continuous cool gel layer and a sandwich fabric, wherein the bottom end of the continuous cool gel layer is connected to the top end of the sandwich fabric.

[0023] Preferably, the breathable sandwich fabric has a grammage between 100 g / m2 and 1000 g / m2.

[0024] Preferably, the sandwich fabric includes a surface silk layer, a supporting breathable layer and a bottom silk layer, the bottom end of the continuous cooling gel layer is connected to the top end of the surface silk layer, the bottom end of the surface silk layer is connected to the top end of the supporting breathable layer, and the top end of the bottom silk layer is connected to the bottom end of the supporting breathable layer.

[0025] Preferably, the supporting breathable layer has a loose breathable mesh structure.

[0026] The application of the novel continuous cool breathable fabric of the present invention can be used in the textile fabric or clothing industry, and is also suitable for printing, coating and impregnation processing in the fields of sponge, paper, rubber and plastic.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. Use sodium bisulfite compounds to first block the isocyanate, then mix and treat it with compounds containing carboxylic acid groups or polyether polyol compounds before curing, unblock it after high-temperature heating, and the two undergo a curing reaction to form a continuous cool gel film, which will be applied to the textile field;

[0029] 2. The sandwich fabric is used in combination with the continuous cooling gel film to improve the heat absorption and cooling effect of the fabric;

[0030] 3. Through the process in step 1, the difficulty of curing control of printing and dyeing materials containing isocyanate is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the structure of the present invention;

[0032] Figure 2 1 is a schematic diagram of a continuous cooling temperature change curve of a comparative test of Example 1 of the present invention;

[0033] Figure 3 1 is a schematic diagram of a continuous cooling temperature change curve of a comparative test of Example 2 of the present invention;

[0034] Figure 4 1 is a schematic diagram of a continuous cooling temperature change curve of a comparative test of Example 3 of the present invention;

[0035] Figure 5 1 is a schematic diagram of a continuous cooling temperature change curve of a comparative test of Example 4 of the present invention;

[0036] Figure 6 is a schematic diagram of a continuous cooling temperature change curve of a comparative test of Example 5 of the present invention;

[0037] Figure 7 is a schematic diagram of a continuous cooling temperature change curve of a comparative test of Example 6 of the present invention;

[0038] Figure 8 is a schematic diagram of a continuous cooling temperature change curve of a comparative test of Example 7 of the present invention;

[0039] Markings in the attached figure: 1. continuous cooling gel layer; 2. surface silk layer; 3. supporting breathable layer; 4. bottom silk layer. DETAILED DESCRIPTION

[0040] In order to facilitate understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0041] like Figures 1 to 8 As shown:

[0042] Example 1

[0043] S1. Weigh 50 parts by weight of deionized water, slowly add 50 parts by weight of solid sodium bisulfite, and completely dissolve it under stirring;

[0044] S2, weigh 200 parts by mass of 330N isocyanate, slowly add it into the S1 solution, stir evenly for 40 minutes at a temperature below 35°C to perform end-capping treatment;

[0045] S3, weigh 80 parts by mass of polyether polyol of model 5065 and 0.2 parts by mass of catalysts of models A20 and A50, add them, weigh 19.5 parts by mass of the mixture prepared in S2, mix them, add appropriate amount of deionized water, adjust to a viscosity suitable for printing, stir evenly for 30 minutes at a temperature below 35°C, and let stand for 60 minutes to degas for use;

[0046] S4, take 100 meters of sandwich fabric with a weight of 190 g / m2, use a flat screen printing machine for processing, the printing pattern is full-ground printing, pour the pre-treated mixture in S3 into a slurry barrel, print on the sandwich fabric, first pre-bake, set the oven temperature to 110°C, the oven length to 40 meters, pass through the oven at a speed of 10 meters / second to dry the fabric, then bake the printed surface, set the oven temperature to 130°C, the oven length to 40 meters, pass through the oven at a speed of 8 meters / second to dry the printed surface to form a film, and thus obtain a gel-coated sandwich fabric with polyurethane as a film-forming material and a significant continuous cooling function;

[0047] S5. Use the contact temperature test instrument of Japan DAIEI Company, model KES-F7, in a constant temperature and humidity environment of 20℃ and 65% relative humidity. Place the temperature sensor on the electric heating plate and raise its temperature to 40℃, with a temperature difference of 20℃ from the ambient temperature. At the same time, place the test sample on another heating plate, which is set to the same temperature as the ambient temperature of 20℃. After the temperature sensor is constant at 40℃, quickly move the temperature sensor to the test sample and test the temperature change of the sensor for 3 minutes. The instrument automatically records the test results every 0.1s.

[0048] S6. Using the test method in step S5, the gel processed product prepared in step S4 is tested and compared with the product without gel processing. The temperature-time variation curve ( Figure 2 );

[0049] Select the same detection time point, the instrument records the temperature changes of the gel processed product and the non-gel processed product, and the comparison is as follows:

[0050] Comparison 1#Test product Temperature difference 0 40 40 0 2 39.89 39.88 0.01 4 39.28 38.82 0.46 6 39.03 38.28 0.75 8 38.82 37.78 1.04 10 38.6 37.81 0.79 14 38.29 37.34 0.95 18 38.01 36.98 1.03 24 37.46 36.51 0.95 30 36.99 36 0.99 60 34.85 34.01 0.84 90 33.04 32.31 0.73 120 31.45 30.79 0.66 180 28.78 28.35 0.43 240 26.77 26.46 0.31 300 25.21 25.05 0.16

[0051] As can be seen from the table, the maximum temperature difference between the gel-processed product and the unprocessed product is 1.03°C, and the temperature difference lasts for more than 3 minutes, which has a continuous cooling effect, but the continuous cooling function is not obvious.

[0052] Example 2

[0053] S1. Weigh 100 parts by mass of deionized water, slowly add 100 parts by mass of solid sodium bisulfite, and completely dissolve it under stirring;

[0054] S2, weigh 200 parts by mass of 330N isocyanate, slowly add it into the S1 solution, stir evenly for 40 minutes at a temperature below 35°C to perform end-capping treatment;

[0055] S3, weigh 80 parts by mass of polyether polyol of model 5065 and 0.2 parts by mass of catalysts of models A20 and A50, add them, weigh 19.5 parts by mass of the mixture prepared in S2, mix them, add appropriate amount of deionized water, adjust to a viscosity suitable for printing, stir evenly for 30 minutes at a temperature below 35°C, and let stand for 60 minutes to degas for use;

[0056] S4, take 100 meters of sandwich fabric with a weight of 190 g / m2, use a flat screen printing machine for processing, the printing pattern is full-ground printing, pour the pre-treated mixture in S3 into a slurry barrel, print on the sandwich fabric, first pre-bake, set the oven temperature to 110°C, the oven length to 40 meters, pass through the oven at a speed of 10 meters / second to dry the fabric, then bake the printed surface, set the oven temperature to 130°C, the oven length to 40 meters, pass through the oven at a speed of 8 meters / second to dry the printed surface to form a film, and thus obtain a gel-coated sandwich fabric with polyurethane as a film-forming material and a significant continuous cooling function;

[0057] S5. Using the test method in the above embodiment 1, the gel processed product prepared in S4 was tested and compared with the product without gel processing. The temperature-time variation curve ( Figure 3 );

[0058] Select the same detection time point, the instrument records the temperature changes of the gel processed product and the non-gel processed product, and the comparison is as follows:

[0059]

[0060]

[0061] As can be seen from the table, the maximum temperature difference between the gel-processed product and the unprocessed product is 4.92°C, and the temperature difference of 1°C lasts for more than 3 minutes, which has a continuous and obvious cooling effect and a continuous cooling function.

[0062] Example 3

[0063] S1. Weigh 100 parts by mass of deionized water, slowly add 100 parts by mass of solid sodium bisulfite, and completely dissolve it under stirring;

[0064] S2, weigh 50 parts by mass of 330N isocyanate, slowly add it into the S1 solution, stir evenly for 40 minutes at a temperature below 35°C to perform end-capping treatment;

[0065] S3, weigh 80 parts by mass of polyether polyol of model 5065 and 0.2 parts by mass of catalysts of models A20 and A50, add them, weigh 19.5 parts by mass of the mixture prepared in S2, mix them, add appropriate amount of deionized water, adjust to a viscosity suitable for printing, stir evenly for 30 minutes at a temperature below 35°C, and let stand for 60 minutes to degas for use;

[0066] S4, take 100 meters of sandwich fabric with a weight of 190 g / m2, use a flat screen printing machine for processing, the printing pattern is full-ground printing, pour the pre-treated mixture in S3 into a slurry barrel, print on the sandwich fabric, first pre-bake, set the oven temperature to 110°C, the oven length to 40 meters, pass through the oven at a speed of 10 meters / second to dry the fabric, then bake the printed surface, set the oven temperature to 130°C, the oven length to 40 meters, pass through the oven at a speed of 8 meters / second to dry the printed surface to form a film, and thus obtain a gel-coated sandwich fabric with polyurethane as a film-forming material and a significant continuous cooling function;

[0067] S5. Using the test method in the above embodiment 1, the gel processed product obtained in step S4 is tested, and a temperature-time variation curve is plotted ( Figure 4 );

[0068] Select the same detection time point, the instrument records the temperature changes of the gel processed product and the non-gel processed product, and the comparison is as follows:

[0069]

[0070]

[0071] As can be seen from the table, the maximum temperature difference between the gel-processed product and the unprocessed product is 1.95°C, and the temperature difference lasts for more than 3 minutes, which has a continuous cooling effect, but the continuous cooling function is not obvious.

[0072] By comparing specific examples 1, 2, and 3, it can be seen that when other conditions remain unchanged and only the mass fraction ratio of sodium bisulfite to isocyanate is changed, the cooling effect is very different. The reasons are analyzed. In specific example 1, the molar number of HSO3- in the sodium bisulfite solution is insufficient, resulting in insufficient end-capping of the isocyanate. After unblocking, the reaction with the polyether polyol is insufficient, and a small amount of gel is generated. Therefore, the cooling effect is not ideal. In specific example 3, due to the insufficient molar number of the isocyanate group -NCO, the reaction is insufficient. In the mixture, a large amount of free bisulfite ions and sodium ions are mixed, which affects the reaction of the isocyanate with the polyether polyol after unblocking, and a small amount of gel is generated. Therefore, the cooling effect is also not ideal. In specific example 2, the HSO3:NCO molar ratio is 1.2:1, and the sodium bisulfite reacts fully with the isocyanate and is completely end-capped. After heating and unblocking, it fully reacts with the polyether polyol to generate a gel. Therefore, the optimal reaction molar ratio of HSO3:NCO is 1-1.2:1

[0073] Example 4

[0074] S1. Weigh 100 parts by mass of deionized water, slowly add 100 parts by mass of solid sodium bisulfite, and completely dissolve it under stirring;

[0075] S2. Weigh 200 parts by mass of 330N isocyanate, slowly add it into the S1 solution, stir evenly for 40 minutes at a temperature below 35°C to perform end-capping treatment.

[0076] S3, weigh 60 parts by mass of polyether polyol of model 5065 and 0.2 parts by mass of catalysts of models A20 and A50, add them, weigh 39.5 parts by mass of the mixture prepared in S2, mix them, add appropriate amount of deionized water, adjust to a viscosity suitable for printing, stir evenly for 30 minutes at a temperature below 35°C, and let stand for 60 minutes to degas for use;

[0077] S5, take 100 meters of sandwich fabric with a weight of 190 g / m2, use a flat screen printing machine for processing, the printing pattern is full-ground printing, pour the pre-treated mixture in S4 into a slurry barrel, print on the sandwich fabric, first pre-bake, set the oven temperature to 110°C, the oven length to 40 meters, pass through the oven at a speed of 10 meters / second to dry the fabric, then bake the printed surface, set the oven temperature to 130°C, the oven length to 40 meters, pass through the oven at a speed of 8 meters / second to dry the printed surface to form a film, and thus obtain a gel-coated sandwich fabric with polyurethane as the film-forming material and a significant continuous cooling function;

[0078] S6. Using the test method in the first embodiment, the gel processed product obtained in step S5 is tested and compared with the product without gel processing. The temperature-time variation curve ( Figure 5 );

[0079] Select the same detection time point, the instrument records the temperature changes of the gel processed product and the non-gel processed product, and the comparison is as follows:

[0080]

[0081] As can be seen from the table, the maximum temperature difference between the gel-processed product and the unprocessed product is 3.05°C, and the temperature difference lasts for more than 3 minutes, which has a continuous and obvious cooling effect and a continuous cooling function.

[0082] Example 5

[0083] S1. Weigh 100 parts by mass of deionized water, slowly add 100 parts by mass of solid sodium bisulfite, and completely dissolve it under stirring;

[0084] S2, weigh 200 parts by mass of 330N isocyanate, slowly add it into the S1 solution, stir evenly for 40 minutes at a temperature below 35°C to perform end-capping treatment;

[0085] S3, weigh 75 parts by mass of polyether polyol of model 5065 and 0.2 parts by mass of catalysts of models A20 and A50, add them thereto, weigh 24.5 parts by mass of the mixture prepared in S3, mix them, add appropriate amount of deionized water, adjust to a viscosity suitable for printing, stir evenly for 30 minutes at a temperature below 35°C, and let stand for 60 minutes to degas for use;

[0086] S4, take 100 meters of sandwich fabric with a weight of 190 g / m2, use a flat screen printing machine for processing, the printing pattern is full-ground printing, pour the pre-treated mixture in S3 into a slurry barrel, print on the sandwich fabric, first pre-bake, set the oven temperature to 110°C, the oven length to 40 meters, pass through the oven at a speed of 10 meters / second to dry the fabric, then bake the printed surface, set the oven temperature to 130°C, the oven length to 40 meters, pass through the oven at a speed of 8 meters / second to dry the printed surface to form a film, and thus obtain a gel-coated sandwich fabric with polyurethane as a film-forming material and a significant continuous cooling function;

[0087] S5. Using the test method in the first embodiment, the gel processed product prepared in S4 is tested and compared with the product without gel processing. The temperature-time variation curve ( Figure 6 );

[0088] Select the same detection time point, the instrument records the temperature changes of the gel processed product and the non-gel processed product, and the comparison is as follows:

[0089]

[0090]

[0091] As can be seen from the table, the maximum temperature difference between the gel-processed product and the unprocessed product is 4.1°C, and the temperature difference lasts for more than 3 minutes, with a sustained and significant cooling effect and a significant continuous cooling function.

[0092] Example 6

[0093] S1. Weigh 100 parts by mass of deionized water, slowly add 100 parts by mass of solid sodium bisulfite, and completely dissolve it under stirring;

[0094] S2, weigh 200 parts by mass of 330N isocyanate, slowly add it into the S1 solution, stir evenly for 40 minutes at a temperature below 35°C to perform end-capping treatment;

[0095] S3, weigh 70 parts by mass of polyether polyol of model 5065 and 0.2 parts by mass of catalysts of models A20 and A50, add them thereto, weigh 29.5 parts by mass of the mixture prepared in S2, mix them, add appropriate amount of deionized water, adjust to a viscosity suitable for printing, stir evenly for 30 minutes at a temperature below 35°C, and let stand for 60 minutes to degas for use;

[0096] S4, take 100 meters of sandwich fabric with a weight of 190 g / m2, use a flat screen printing machine for processing, the printing pattern is full-ground printing, pour the pre-treated mixture in S3 into a slurry barrel, print on the sandwich fabric, first pre-bake, set the oven temperature to 110°C, the oven length to 40 meters, pass through the oven at a speed of 10 meters / second to dry the fabric, then bake the printed surface, set the oven temperature to 130°C, the oven length to 40 meters, pass through the oven at a speed of 8 meters / second to dry the printed surface to form a film, and thus obtain a gel-coated sandwich fabric with polyurethane as a film-forming material and a significant continuous cooling function;

[0097] S5. Using the test method in the first embodiment, the gel processed product prepared in S4 is tested and compared with the product without gel processing. The temperature-time variation curve ( Figure 7 );

[0098] Select the same detection time point, the instrument records the temperature changes of the gel processed product and the non-gel processed product, and the comparison is as follows:

[0099]

[0100]

[0101] As can be seen from the table, the maximum temperature difference between the gel-processed product and the unprocessed product is 6.03°C, and there is a continuous temperature difference of 2°C, which lasts for more than 3 minutes. It has a continuous and obvious cooling effect, and the continuous cooling function is very obvious.

[0102] By comparing specific examples 4, 5, and 6, it can be seen that other conditions remain unchanged, only the mass fraction ratio of polyether polyol to isocyanate is changed, and the cooling effect is tested to be very different. The reasons are analyzed. In specific example 6, isocyanate accounts for 50% of the mixture, and a mixture with a mass fraction of 29.5 is used, the isocyanate dosage is converted to 14.5, and a polyether polyol mass fraction of 70 is used. The ratio of the two is close to 100:20, and the two react fully to generate a large amount of gel, the cooling effect is obvious, and the continuous cooling function is obvious. In specific examples 4 and 5, the mass fraction ratio of polyether polyol to isocyanate deviates from the full reaction ratio. After the isocyanate end-capping is heated and unblocked, it does not react fully with the polyether polyol, and less gel is generated, so the cooling effect is not ideal. Therefore, the mass fraction ratio of polyether polyol to isocyanate is 100:15-25.

[0103] Example 7

[0104] S1. Weigh 100 parts by mass of deionized water, slowly add 100 parts by mass of solid sodium bisulfite, and completely dissolve it under stirring;

[0105] S2, weigh 200 parts by mass of 330N isocyanate, slowly add it into the S1 solution, stir evenly for 40 minutes at a temperature below 35°C to perform end-capping treatment;

[0106] S3, weigh 60 parts by mass of polyether polyol of model 5065 and 0.2 parts by mass of catalysts of models A20 and A50, add them, weigh 39.5 parts by mass of the mixture prepared in S2, mix them, add appropriate amount of deionized water, adjust to a viscosity suitable for printing, stir evenly for 30 minutes at a temperature below 35°C, and let stand for 60 minutes to degas for use;

[0107] S4, take 100 meters of sandwich fabric with a weight of 190 g / m2, use a flat screen printing machine for processing, the printing pattern is full-ground printing, pour the pre-treated mixture in S3 into a slurry barrel, print on the sandwich fabric, first pre-bake, set the oven temperature to 120°C, the oven length to 40 meters, pass through the oven at a speed of 10 meters / second to dry the fabric, then bake the printed surface, set the oven temperature to 150°C, the oven length to 40 meters, pass through the oven at a speed of 8 meters / second to dry the printed surface to form a film, and thus obtain a gel-coated sandwich fabric with polyurethane as a film-forming material and a significant continuous cooling function;

[0108] S5. Using the test method in the above embodiment 1, the gel processed product prepared in S4 was tested and compared with the product without gel processing. The temperature-time variation curve ( Figure 8 );

[0109] Select the same detection time point, the instrument records the temperature changes of the gel processed product and the non-gel processed product, and the comparison is as follows:

[0110]

[0111] As can be seen from the table, the maximum temperature difference between the gel processed product and the unprocessed product is 3.51℃, and the temperature difference lasts for more than 3 minutes, which has a continuous and obvious cooling effect and a continuous cooling function;

[0112] By comparing specific embodiments 4 and 7, it can be seen that when other conditions remain unchanged and only the drying temperature is changed, the test cooling effect does not change much. Therefore, although the drying temperature affects the gel formation, resulting in a slight difference in the test temperature difference, the influencing factor is small. The optimal drying conditions are: pre-baking at a temperature of 100-120°C and a drying time of 3-6 minutes, and then baking at a temperature of 130°-150°C and a time of 5-10 minutes.

[0113] In summary, the optimal reaction conditions are: the mass ratio of sodium bisulfate to isocyanate, with the HSO3:NCO molar ratio of 1-1.2:1 being the best, the mass ratio of polyether polyol to isocyanate being 100:15-25 for full reaction, and the optimal drying conditions: pre-baking at a temperature of 100-120°C for 3-6 minutes, and then baking at a temperature of 130°-150°C for 5-10 minutes.

[0114] Technical personnel in this industry only need to operate according to the accompanying instruction manual, and there is no need for technical personnel in this field to make creative efforts.

[0115] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a novel continuous cool breathable fabric. It is characterized in that The following steps are involved: Step 1: Preparation of continuous cooling gel The isocyanate used is blocked with sodium bisulfite, and then the blocked isocyanate is pre-cured with a compound containing a carboxylic acid group or a polyether polyol compound to make the isocyanate resin gel curing process controllable, and then allowed to stand for 60 minutes to degas for use; Step 2: Sandwich fabric preparation A surface silk layer, a supporting breathable layer and a bottom silk layer are prepared by using a knitting machine, and the surface silk layer is located on the supporting breathable layer, and the supporting breathable layer is located between the surface silk layer and the bottom silk layer to form a sandwich fabric; Step 3: Printing, coating and impregnation A printing machine is used to perform printing, coating and impregnation processes on the top surface of the sandwich fabric surface silk layer, and the continuous cooling gel is printed on the top surface of the sandwich fabric surface silk layer; Step 4: Molding Pre-baking is performed at a temperature of 100-140°C for 3-10 minutes, and then baking is performed at a temperature of 130°-160°C for 5-15 minutes to unblock the blocked isocyanate, and the printed and dyed surface containing carboxylic acid compounds or polyether polyol compounds is cured to form a thermosetting continuous cooling gel coating layer of the continuous cooling gel, thereby forming a coated gel sandwich fabric with significant continuous cooling function; Step 5: Packaging Packing and warehousing of finished fabrics; In the step 1, the molar ratio of sodium bisulfite to isocyanate is 1-1.2:1, and the molar ratio of polyether polyol to isocyanate is 100:15-25.

2. A method for preparing a novel continuous cool breathable fabric as claimed in claim 1, It is characterized in that In the step 2, the surface silk layer is composed of 2 polyester fully stretched filaments FDY with a fineness between 50D-500D, the supporting breathable layer is composed of polyester fully stretched monofilament FDY with a fineness between 24D-300D, and the bottom silk layer is composed of polyester fully stretched filament FDY with a fineness between 50D-500D.

3. A method for preparing a novel continuous cool breathable fabric as claimed in claim 1, It is characterized in that The isocyanate in the step 1 can be aliphatic isocyanate, aromatic isocyanate or a mixture of aliphatic isocyanate and aromatic isocyanate in any proportion.

4. A method for preparing a novel continuous cool breathable fabric as claimed in claim 1, It is characterized in that The isocyanate system in step 1 is hydrophilic and soluble in aqueous solution.

5. A method for preparing a novel continuous cool breathable fabric as claimed in claim 1, It is characterized in that In the step 4, pre-baking is performed at a temperature of 100-120° C. for 3-6 minutes, and then baking is performed at a temperature of 130°-150° C. for 5-10 minutes.

6. A new type of continuously cool breathable fabric, It is characterized in that The invention comprises a continuous cooling gel layer (1) and a sandwich fabric, wherein the bottom end of the continuous cooling gel layer (1) is connected to the top end of the sandwich fabric, and the sandwich fabric comprises a surface silk layer (2), a supporting breathable layer (3) and a bottom silk layer (4), wherein the bottom end of the continuous cooling gel layer (1) is connected to the top end of the surface silk layer (2), the bottom end of the surface silk layer (2) is connected to the top end of the supporting breathable layer (3), and the top end of the bottom silk layer (4) is connected to the bottom end of the supporting breathable layer (3).

7. Application of a novel continuous cool breathable fabric, wherein the novel continuous cool breathable fabric is prepared by the preparation method according to any one of claims 1 to 5. It is characterized in that It can be used in textile fabric or clothing industry, and is also suitable for printing, coating and impregnation processing in sponge, paper, rubber and plastic fields.

Citation Information

Patent Citations

  • A breathable sports fabric

    CN113290960B

  • High-strength photo-cured and thermal-cured polyurethane adhesive as well as preparation method and application method thereof

    CN108395847A

  • Preparation method of heat-preservation and heat-insulation tent composite fabric

    CN110481105A