A new additive material for reducing the rebound rate of tunnel wet shotcrete
Through the coordination of modified basalt fiber and composite powder, the problems of high rebound rate and insufficient early strength of wet shotcrete are solved, the effect of reducing the rebound rate and the amount of accelerator is achieved, and the construction cost is reduced.
Patent Information
- Application Number
- CN202310228946.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2043-03-10
AI Technical Summary
The existing wet shotcrete has a high rebound rate, insufficient early strength, and high dependence on accelerators, resulting in increased construction costs.
A new type of additive material is used with modified basalt fiber as the skeleton and composite powder as the admixture. Through modification and grinding, the synergistic performance of the fiber and powder is enhanced, and the rebound rate and the amount of accelerator are reduced.
While ensuring early strength, it significantly reduces the rebound rate of wet shotcrete and the amount of accelerator, saving costs and improving construction efficiency.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wet sprayed concrete, and in particular to a novel additive material for reducing the rebound rate of tunnel wet sprayed concrete. Background Art
[0002] Shotcrete is a type of concrete that is made by using a spraying machine, compressed air or other power to transport a certain proportion of mixed materials through a pipeline and spray them at high speed onto the sprayed surface (rock surface, formwork, old buildings, etc.) to solidify and harden. Currently, it is mainly used in tunnel construction. Shotcrete has the advantages of timely support, high strength, strong density, relatively simple and flexible operation, etc., especially under soft surrounding rock geological conditions, with steel arch frame and system anchor as joint support, its advantages are more significant.
[0003] The spraying construction process of tunnel shotcrete is mainly divided into dry spraying and wet spraying. The dry spraying method is a method in which cement, sand and stone are mixed evenly in a dry state, and then compressed air is used to send them and the accelerator to the nozzle and spray them after mixing with pressurized water. Its advantages are convenient construction and low engineering cost. Its disadvantages are low construction efficiency, high labor intensity, poor quality resulting in high rebound rate, large dust and harsh environment during on-site construction; the wet spraying method is a method in which the mixed concrete is sent to the nozzle through a grouting pump and then sprayed with compressed air. Its advantages are easy to control the quality of concrete, low rebound, high construction efficiency and relatively good working environment. Its disadvantages are high construction space requirements and high equipment and material costs. Therefore, wet spraying is generally used for construction.
[0004] Even if the wet spraying method is chosen for construction, there are still some problems to be improved and solved. Due to the large number of accelerator manufacturers on the market, the product quality and actual use effects are also uneven. Such as insufficient early strength, compatibility issues with water reducers, corrosive issues of alkaline accelerators, and the fact that accelerators from different manufacturers and types generally cannot be mixed. In addition, although the promotion and application of accelerators has solved the main support problems of tunnel construction, if the rebound rate is to reach a relatively ideal state, the selection of accelerators is particularly important, and the single dosage also needs to be large. Therefore, excessive reliance on accelerators also invisibly increases the cost of the construction party. In response to the above problems, the relevant research on how to further effectively reduce the rebound rate of wet spraying concrete has attracted the attention and thinking of industry personnel. It mainly focuses on how to effectively reduce the rebound rate of wet spraying concrete without increasing costs. Summary of the invention
[0005] In view of the defects of the prior art, the purpose of the present invention is to provide a new additive material for reducing the rebound rate of tunnel wet spraying concrete, so as to solve the problems raised in the above background technology.
[0006] The present invention solves the technical problem by adopting the following technical solution:
[0007] The invention provides a new additive material for reducing the rebound rate of tunnel wet spraying concrete. The new additive material is a new additive material composed of modified basalt fiber as a skeleton and composite powder as an admixture.
[0008] Preferably, the modification method of the modified basalt fiber is:
[0009] S01: Add 2-5 parts of chitosan aqueous solution to 10-20 parts of hydrochloric acid, then add 1-3 parts of sodium alkyl sulfonate and 2-5 parts of lanthanum sulfate, stir evenly to obtain a modified solution;
[0010] S02: placing the basalt fiber in 3-5 times the modification liquid and stirring for modification treatment, the stirring modification speed is 500-1000r / min, the stirring time is 20-30min, and after the stirring is completed, washing and drying are performed to obtain modified basalt fiber.
[0011] Preferably, the mass fraction of the chitosan aqueous solution is 10-20%.
[0012] Preferably, after the SO2 basalt fiber is stirred and modified, it is further ground by adding 1-5% of the total amount of the basalt fiber in an abrasive, and after the grinding is completed, it is washed with water and dried;
[0013] The preparation method of the abrasive is as follows:
[0014] Bentonite is added to a 10% by mass sodium alginate aqueous solution at a weight ratio of 1:5, and then a silane coupling agent is added in an amount of 2-5% of the total amount of bentonite, and the mixture is stirred evenly to obtain an abrasive.
[0015] Preferably, the mass fraction of the sodium alginate aqueous solution is 10-20%.
[0016] Preferably, the silane coupling agent is coupling agent KH560.
[0017] Preferably, the grinding process has a rotation speed of 500-1000 r / min and a grinding time of 20-30 min.
[0018] Preferably, the basalt fiber has a length of 15-30 mm and a diameter of 9-25 μm; wherein the modified basalt fiber accounts for 1-5% of the new additive material.
[0019] Preferably, the preparation method of the composite powder is:
[0020] Add 2-5 parts of silica sol to 10-15 parts of ethanol, then add 1-3 parts of dopamine hydrochloride solution and 2-4 parts of graphene, stir evenly, then wash with water and dry to obtain a composite powder.
[0021] Preferably, the mass concentration of the dopamine hydrochloride solution is 1-1.5 mol / L.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] Aiming at the problems of large rebound rate and insufficient early strength of current wet sprayed concrete, the present invention provides a new composite additive material which can effectively reduce the rebound rate of tunnel wet sprayed concrete, which is composed of basalt fiber and a composite powder. While ensuring the early strength of sprayed concrete, it can achieve the effect of reducing the amount of accelerator and rebound rate to a certain extent, saving costs. The basalt fiber is modified and matched with the composite powder, and the raw materials are coordinated with each other to enhance the performance of the product. Implementation
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0025] The present embodiment provides a new additive material for reducing the rebound rate of tunnel wet sprayed concrete. The new additive material is a new additive material composed of modified basalt fiber as a skeleton and composite powder as an admixture.
[0026] The modification method of the modified basalt fiber in this embodiment is:
[0027] S01: Add 2-5 parts of chitosan aqueous solution to 10-20 parts of hydrochloric acid, then add 1-3 parts of sodium alkyl sulfonate and 2-5 parts of lanthanum sulfate, stir evenly to obtain a modified solution;
[0028] S02: placing the basalt fiber in 3-5 times the modification liquid and stirring for modification treatment, the stirring modification speed is 500-1000r / min, the stirring time is 20-30min, and after the stirring is completed, washing and drying are performed to obtain modified basalt fiber.
[0029] The mass fraction of the chitosan aqueous solution in this embodiment is 10-20%.
[0030] After the SO2 basalt fiber of this embodiment is stirred and modified, it is also ground by adding 1-5% of the total amount of basalt fiber to the grinding agent, and after the grinding is completed, it is washed with water and dried;
[0031] The preparation method of the abrasive is as follows:
[0032] Bentonite is added to a 10% by mass sodium alginate aqueous solution at a weight ratio of 1:5, and then a silane coupling agent is added in an amount of 2-5% of the total amount of bentonite, and the mixture is stirred evenly to obtain an abrasive.
[0033] The mass fraction of the sodium alginate aqueous solution in this embodiment is 10-20%.
[0034] The silane coupling agent in this embodiment is coupling agent KH560.
[0035] The grinding speed of this embodiment is 500-1000r / min, and the grinding time is 20-30min.
[0036] The specifications of the basalt fiber in this embodiment are 15-30 mm in length and 9-25 μm in diameter; the modified basalt fiber accounts for 1-5% of the new additive material.
[0037] The preparation method of the composite powder of this embodiment is:
[0038] Add 2-5 parts of silica sol to 10-15 parts of ethanol, then add 1-3 parts of dopamine hydrochloride solution and 2-4 parts of graphene, stir evenly, then wash with water and dry to obtain a composite powder.
[0039] The mass concentration of the dopamine hydrochloride solution in this embodiment is 1-1.5 mol / L. Example
[0040] The present embodiment provides a new additive material for reducing the rebound rate of tunnel wet sprayed concrete. The new additive material is a new additive material composed of modified basalt fiber as a skeleton and composite powder as an admixture.
[0041] The modification method of the modified basalt fiber in this embodiment is:
[0042] S01: Add 2 parts of chitosan aqueous solution to 10 parts of hydrochloric acid, then add 1 part of sodium alkyl sulfonate and 2 parts of lanthanum sulfate, stir evenly to obtain a modified solution;
[0043] S02: placing the basalt fiber in 3 times the modification liquid and stirring for modification treatment, the stirring modification speed is 500r / min, the stirring time is 20min, and after the stirring is completed, washing and drying are performed to obtain modified basalt fiber.
[0044] The mass fraction of the chitosan aqueous solution in this embodiment is 10%.
[0045] After the S02 basalt fiber of this embodiment is stirred and modified, it is also ground by adding 1% of the total amount of basalt fiber to the grinding agent, and after the grinding is completed, it is washed with water and dried;
[0046] The preparation method of the abrasive is as follows:
[0047] Bentonite was added into a 10% by mass sodium alginate aqueous solution at a weight ratio of 1:5, and then a silane coupling agent of 2% of the total amount of bentonite was added, and the mixture was stirred evenly to obtain an abrasive.
[0048] The mass fraction of the sodium alginate aqueous solution in this embodiment is 10%
[0049] The silane coupling agent in this embodiment is coupling agent KH560.
[0050] The grinding speed of this embodiment is 500 r / min, and the grinding time is 20 min.
[0051] The specifications of the basalt fiber in this embodiment are 10 mm in length and 9 μm in diameter; the modified basalt fiber accounts for 1% of the new additive material.
[0052] The preparation method of the composite powder of this embodiment is:
[0053] 2 parts of silica sol are added to 10 parts of ethanol, and then 1 part of dopamine hydrochloride solution and 2 parts of graphene are added, stirred evenly, and then washed with water and dried to obtain a composite powder.
[0054] The mass concentration of the dopamine hydrochloride solution in this embodiment is 1 mol / L. Example
[0055] The present embodiment provides a new additive material for reducing the rebound rate of tunnel wet sprayed concrete. The new additive material is a new additive material composed of modified basalt fiber as a skeleton and composite powder as an admixture.
[0056] The modification method of the modified basalt fiber in this embodiment is:
[0057] S01: Add 5 parts of chitosan aqueous solution to 20 parts of hydrochloric acid, then add 3 parts of sodium alkyl sulfonate and 5 parts of lanthanum sulfate, stir evenly to obtain a modified solution;
[0058] S02: placing the basalt fiber in 5 times the modification liquid and stirring for modification treatment, the stirring modification speed is 1000r / min, the stirring time is 30min, and after the stirring is completed, washing and drying are performed to obtain modified basalt fiber.
[0059] The mass fraction of the chitosan aqueous solution in this embodiment is 20%.
[0060] After the S02 basalt fiber of this embodiment is stirred and modified, it is also ground by adding 5% of the total amount of basalt fiber. After the grinding is completed, it is washed with water and dried.
[0061] The preparation method of the abrasive is as follows:
[0062] Bentonite was added into a 10% by mass sodium alginate aqueous solution at a weight ratio of 1:5, and then a silane coupling agent of 5% of the total amount of bentonite was added, and the mixture was stirred evenly to obtain an abrasive.
[0063] The mass fraction of the sodium alginate aqueous solution in this embodiment is 20%
[0064] The silane coupling agent in this embodiment is coupling agent KH560.
[0065] The grinding speed of this embodiment is 1000 r / min, and the grinding time is 30 min.
[0066] The specifications of the basalt fiber in this embodiment are 30 mm in length and 25 μm in diameter; the modified basalt fiber accounts for 5% of the new additive material.
[0067] The preparation method of the composite powder of this embodiment is:
[0068] 5 parts of silica sol were added to 15 parts of ethanol, and then 3 parts of dopamine hydrochloride solution and 4 parts of graphene were added, stirred evenly, and then washed with water and dried to obtain a composite powder.
[0069] The mass concentration of the dopamine hydrochloride solution in this embodiment is 1.5 mol / L. Example
[0070] The present embodiment provides a new additive material for reducing the rebound rate of tunnel wet sprayed concrete. The new additive material is a new additive material composed of modified basalt fiber as a skeleton and composite powder as an admixture.
[0071] The modification method of the modified basalt fiber in this embodiment is:
[0072] S01: Add 3.5 parts of chitosan aqueous solution to 15 parts of hydrochloric acid, then add 2 parts of sodium alkyl sulfonate and 3.5 parts of lanthanum sulfate, stir evenly to obtain a modified solution;
[0073] S02: placing the basalt fiber in 4 times the modification liquid and stirring for modification treatment, the stirring modification speed is 750r / min, the stirring time is 25min, and after the stirring is completed, washing and drying are performed to obtain modified basalt fiber.
[0074] The mass fraction of the chitosan aqueous solution in this embodiment is 15%.
[0075] After the S02 basalt fiber of this embodiment is stirred and modified, it is also ground by adding 3% of the total amount of basalt fiber. After the grinding is completed, it is washed with water and dried.
[0076] The preparation method of the abrasive is as follows:
[0077] Bentonite was added into a 10% by mass sodium alginate aqueous solution at a weight ratio of 1:5, and then a silane coupling agent of 3.5% of the total amount of bentonite was added, and the mixture was stirred evenly to obtain an abrasive.
[0078] The mass fraction of the sodium alginate aqueous solution in this embodiment is 12%.
[0079] The silane coupling agent in this embodiment is coupling agent KH560.
[0080] The grinding speed of this embodiment is 600 r / min, and the grinding time is 22 min.
[0081] The specifications of the basalt fiber in this embodiment are 18 mm in length and 12 μm in diameter; the modified basalt fiber accounts for 2% of the new additive material.
[0082] The preparation method of the composite powder of this embodiment is:
[0083] 3 parts of silica sol were added to 12 parts of ethanol, and then 2 parts of dopamine hydrochloride solution and 3 parts of graphene were added, stirred evenly, and then washed with water and dried to obtain a composite powder.
[0084] The mass concentration of the dopamine hydrochloride solution in this embodiment is 1.2 mol / L. Example
[0085] The present embodiment provides a new additive material for reducing the rebound rate of tunnel wet sprayed concrete. The new additive material is a new additive material composed of modified basalt fiber as a skeleton and composite powder as an admixture.
[0086] The modification method of the modified basalt fiber in this embodiment is:
[0087] S01: Add 4 parts of chitosan aqueous solution to 18 parts of hydrochloric acid, then add 2.9 parts of sodium alkyl sulfonate and 4 parts of lanthanum sulfate, stir evenly to obtain a modified solution;
[0088] S02: placing the basalt fiber in 4 times the modification liquid and stirring for modification treatment, the stirring modification speed is 780r / min, the stirring time is 28min, and after the stirring is completed, washing and drying are performed to obtain modified basalt fiber.
[0089] The mass fraction of the chitosan aqueous solution in this embodiment is 18%.
[0090] After the SO2 basalt fiber of this embodiment is stirred and modified, it is also ground by adding 1-5% of the total amount of basalt fiber to the grinding agent, and after the grinding is completed, it is washed with water and dried;
[0091] The preparation method of the abrasive is as follows:
[0092] Bentonite was added into a 10% by mass sodium alginate aqueous solution at a weight ratio of 1:5, and then a silane coupling agent of 4% of the total amount of bentonite was added, and the mixture was stirred evenly to obtain an abrasive.
[0093] The mass fraction of the sodium alginate aqueous solution in this embodiment is 15%.
[0094] The silane coupling agent in this embodiment is coupling agent KH560.
[0095] The grinding speed of this embodiment is 850 r / min, and the grinding time is 28 min.
[0096] The specifications of the basalt fiber in this embodiment are 28 mm in length and 21 μm in diameter; the modified basalt fiber accounts for 4% of the new additive material.
[0097] The preparation method of the composite powder of this embodiment is:
[0098] 4 parts of silica sol were added to 18 parts of ethanol, and then 2 parts of dopamine hydrochloride solution and 3 parts of graphene were added, stirred evenly, and then washed with water and dried to obtain a composite powder.
[0099] The mass concentration of the dopamine hydrochloride solution in this embodiment is 1.4 mol / L. Example
[0100] The present embodiment provides a new additive material for reducing the rebound rate of tunnel wet sprayed concrete. The new additive material is a new additive material composed of modified basalt fiber as a skeleton and composite powder as an admixture.
[0101] The modification method of the modified basalt fiber in this embodiment is:
[0102] S01: Add 4 parts of chitosan aqueous solution to 12 parts of hydrochloric acid, then add 1-3 parts of sodium alkyl sulfonate and 4 parts of lanthanum sulfate, stir evenly to obtain a modified solution;
[0103] S02: placing the basalt fiber in 4 times the modification liquid and stirring for modification treatment, the stirring modification speed is 900r / min, the stirring time is 28min, and after the stirring is completed, washing and drying are performed to obtain modified basalt fiber.
[0104] The mass fraction of the chitosan aqueous solution in this embodiment is 12%.
[0105] After the S02 basalt fiber of this embodiment is stirred and modified, it is also ground by adding 2% of the total amount of basalt fiber. After the grinding is completed, it is washed with water and dried.
[0106] The preparation method of the abrasive is as follows:
[0107] Bentonite was added into a 10% by mass sodium alginate aqueous solution at a weight ratio of 1:5, and then a silane coupling agent of 3% of the total amount of bentonite was added, and the mixture was stirred evenly to obtain an abrasive.
[0108] The mass fraction of the sodium alginate aqueous solution in this embodiment is 18%
[0109] The silane coupling agent in this embodiment is coupling agent KH560.
[0110] The grinding speed of this embodiment is 760r / min, and the grinding time is 24min.
[0111] The basalt fiber specifications of this embodiment are 160 mm in length and 12 μm in diameter; the modified basalt fiber accounts for 2% of the new additive material.
[0112] The preparation method of the composite powder of this embodiment is:
[0113] 3 parts of silica sol were added to 12 parts of ethanol, and then 2 parts of dopamine hydrochloride solution and 3 parts of graphene were added, stirred evenly, and then washed with water and dried to obtain a composite powder.
[0114] The mass concentration of the dopamine hydrochloride solution in this embodiment is 1.2 mol / L. Example
[0115] The present embodiment provides a new additive material for reducing the rebound rate of tunnel wet sprayed concrete. The new additive material is a new additive material composed of modified basalt fiber as a skeleton and composite powder as an admixture.
[0116] The modification method of the modified basalt fiber in this embodiment is:
[0117] S01: Add 5 parts of chitosan aqueous solution to 12 parts of hydrochloric acid, then add 2 parts of sodium alkyl sulfonate and 3 parts of lanthanum sulfate, stir evenly to obtain a modified solution;
[0118] S02: placing the basalt fiber in 3 times the modification liquid and stirring for modification treatment, the stirring modification speed is 600r / min, the stirring time is 22min, and after the stirring is completed, washing and drying are performed to obtain modified basalt fiber.
[0119] The mass fraction of the chitosan aqueous solution in this embodiment is 12%.
[0120] After the S02 basalt fiber of this embodiment is stirred and modified, it is also ground by adding 2% of the total amount of basalt fiber. After the grinding is completed, it is washed with water and dried.
[0121] The preparation method of the abrasive is as follows:
[0122] Bentonite was added into a 10% by mass sodium alginate aqueous solution at a weight ratio of 1:5, and then a silane coupling agent of 3% of the total amount of bentonite was added, and the mixture was stirred evenly to obtain an abrasive.
[0123] The mass fraction of the sodium alginate aqueous solution in this embodiment is 12%
[0124] The silane coupling agent in this embodiment is coupling agent KH560.
[0125] The grinding speed of this embodiment is 550 r / min, and the grinding time is 23 min.
[0126] The basalt fiber specifications of this embodiment are 16 mm in length and 10 μm in diameter; the modified basalt fiber accounts for 2% of the new additive material.
[0127] The preparation method of the composite powder of this embodiment is:
[0128] 3 parts of silica sol were added to 12 parts of ethanol, and then 2 parts of dopamine hydrochloride solution and 3 parts of graphene were added, stirred evenly, and then washed with water and dried to obtain a composite powder.
[0129] The mass concentration of the dopamine hydrochloride solution in this embodiment is 1.4 mol / L.
[0130] Comparative Example 1.
[0131] The difference from Example 3 is that the modified basalt fiber is not modified.
[0132] Comparative Example 2.
[0133] The difference from Example 3 is that no modifying liquid treatment is used in the preparation of the modified basalt fiber.
[0134] Comparative Example 3.
[0135] The difference from Example 3 is that the basalt fiber is not treated with an abrasive.
[0136] Comparative Example 4.
[0137] The difference from Example 3 is that no dopamine hydrochloride solution is added during the preparation of the composite powder.
[0138] Comparative Example 5.
[0139] The difference from Example 3 is that talcum powder is used instead of graphene in the preparation of the composite powder.
[0140] The performance measurement results of Examples 1-6 and Comparative Examples 1-5 are as follows
[0141] Rebound rate (%) Example 1 12.9 Example 2 12.8 Example 3 12.1 Example 4 13.2 Example 5 13.3 Example 6 13.1 Comparative Example 1 25.8 Comparative Example 2 24.2 Comparative Example 3 24.5 Comparative Example 4 23.9 Comparative Example 5 23.6
[0142] It can be concluded from Examples 1-3 and Comparative Examples 1-5 that the rebound rate of the product produced by the present invention is significantly reduced, and the method for preparing the modified basalt fiber and the composite powder is unique, and only the method of the present invention can achieve the most significant effect.
[0143] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0144] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An additive material for reducing the rebound rate of tunnel wet sprayed concrete, characterized in that: The additive material is an additive material composed of modified basalt fiber as a skeleton and composite powder as an admixture; the modification method of the modified basalt fiber is: S01: Add 2-5 parts of chitosan aqueous solution to 10-20 parts of hydrochloric acid, then add 1-3 parts of sodium alkyl sulfonate and 2-5 parts of lanthanum sulfate, stir evenly to obtain a modified solution; S02: placing the basalt fiber in a 3-5 times modification liquid and stirring for modification treatment, the stirring modification speed is 500-1000r / min, the stirring time is 20-30min, and after the stirring is completed, washing with water and drying to obtain modified basalt fiber; In step S02, after the basalt fiber is stirred and modified, it is also ground by adding 1-5% of the total amount of the basalt fiber. After the grinding is completed, it is washed with water and dried. The preparation method of the abrasive is as follows: Bentonite is added to a 10% sodium alginate aqueous solution at a weight ratio of 1:5, and then a silane coupling agent is added at a weight ratio of 2-5% of the total amount of bentonite, and the mixture is stirred evenly to obtain an abrasive; The basalt fiber specifications are 15-30 mm in length and 9-25 μm in diameter; The modified basalt fiber accounts for 1-5% of the added materials; the preparation method of the composite powder is: 2-5 parts of silica sol are added to 10-15 parts of ethanol, and then 1-3 parts of dopamine hydrochloride solution and 2-4 parts of graphene are added, stirred evenly, and then washed with water and dried to obtain a composite powder; the mass concentration of the dopamine hydrochloride solution is 1-1.5 mol / L.
2. The additive material for reducing the rebound rate of tunnel wet sprayed concrete according to claim 1, characterized in that: The mass fraction of the chitosan aqueous solution is 10-20%.
3. The additive material for reducing the rebound rate of tunnel wet sprayed concrete according to claim 2, characterized in that: The silane coupling agent is coupling agent KH560.
4. The additive material for reducing the rebound rate of tunnel wet sprayed concrete according to claim 3 is characterized in that: The rotation speed of the grinding process is 500-1000r / min, and the grinding time is 20-30min.