Preparation method and application of side chain cross-linked sulfonated polyarylethersulfoneketone polymer
By using monomers containing sulfonic acid groups and cross-linking agent Z in the proton exchange membrane to perform an amidation reaction, a tight cross-linked network is formed, which solves the problem of the decline in mechanical properties and proton conductivity of existing membranes under high sulfonation degrees. problem, achieving both high conductivity and mechanical properties, and is suitable for fuel cells.
Patent Information
- Application Number
- CN202310296405.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The mechanical properties of existing proton exchange membranes decrease when the degree of sulfonation is high, resulting in swelling or dissolution problems, and the cross-linking method causes a reduction in proton conductivity, making it difficult to meet the requirements of fuel cells for high performance, low cost, and durability.
Monomers containing sulfonic acid groups and cross-linking agent Z are used to perform an amidation reaction under the action of a catalyst to form a tight cross-linked network structure, which improves the swelling resistance and mechanical properties of the membrane while maintaining high proton conductivity.
It achieves both high conductivity and mechanical properties of the proton exchange membrane at high temperatures. The conductivity reaches 0.0678S cm-1-0.0732S cm-1 at 80°C, which significantly improves the heat resistance and dimensional stability of the membrane. .
Smart Images

Figure CN116239805B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of fuel cells and polymer chemistry, and relates to a side chain cross-linked sulfonated polyarylethersulfoneketone proton exchange membrane and a preparation method thereof. Background Art
[0002] With the increasing prominence of energy shortage and environmental pollution, the research and development of fuel cell components has received more and more attention in recent years. As a key material for fuel cells, proton exchange membrane (PEM) needs to meet stringent requirements such as high performance, low cost and durability. DuPont's Nafion series membranes have high proton conductivity, good mechanical properties and excellent stability, but they are also limited by disadvantages such as high preparation cost and high methanol permeability. Sulfonated polyarylethersulfoneketone has high proton conductivity and excellent mechanical strength and is one of the potential PEM candidate materials. The proton conductivity of the membrane mainly depends on the degree of sulfonation. When the degree of sulfonation is low, the proton conductivity of the membrane is low; when the degree of sulfonation is too high, the membrane exhibits high proton conductivity, but its mechanical properties are sharply reduced, causing the membrane to swell or even dissolve in the aqueous medium. Researchers have also tried to overcome the above problems by cross-linking, but the dense network structure after cross-linking significantly reduces the proton conductivity. Summary of the invention
[0003] In order to overcome the problems existing in the above-mentioned prior art, the present invention selects a monomer containing a sulfonic acid group as a crosslinking agent, aiming to prepare a proton exchange membrane with a high degree of sulfonation and high proton conductivity, while also improving its swelling resistance and mechanical properties. The specific measures are: the carboxyl-containing sulfonated polyarylethersulfoneketone and the crosslinking agent Z undergo an amidation reaction under the action of a catalyst, and the formed crosslinked network structure makes the molecular chains become tight, thereby improving the swelling resistance and mechanical properties of the polymer membrane. At the same time, the polymer main chain and the crosslinked network both contain sulfonic acid groups, and the high sulfonic acid group content can improve the proton conductivity of the polymer membrane.
[0004] The present invention is achieved through the following technical solutions:
[0005] A method for preparing a side chain cross-linked sulfonated polyarylethersulfoneketone polymer, wherein the carboxyl-containing sulfonated polyarylethersulfoneketone and a cross-linking agent Z undergo an amidation reaction under the action of a catalyst, and the reaction chemical formula is as follows:
[0006]
[0007] Wherein, x=0.1~0.9, y=0.1~0.9;
[0008] Ar 1 for:
[0009]
[0010] Ar 2 for:
[0011]
[0012] Ar 3 for:
[0013]
[0014] The crosslinking agent Z is:
[0015]
[0016] A method for preparing a side chain cross-linked sulfonated polyarylethersulfoneketone polymer, the specific steps are as follows:
[0017] Step 1: Preparation of carboxyl-containing sulfonated poly(arylethersulfoneketone)
[0018] Under the protection of inert gas, a carboxyl-containing bisphenol monomer, a dihalogen monomer and a sulfonic acid-containing bisphenol monomer are mixed, and then an organic solvent, a water-carrying agent and a salt-forming agent are added. The water-carrying agent carries water at 120-140° C. for 3-6 hours, then the water-carrying agent is discharged, and the temperature is slowly raised to 170-190° C., and the carboxyl-containing sulfonated polyarylethersulfoneketone is obtained after reacting for 15-30 hours.
[0019] Step 2: Add the carboxyl-containing sulfonated polyarylethersulfoneketone obtained in step 1 and the crosslinking agent Z to an organic solvent to obtain a blended liquid, dropwise add the catalyst triphenyl phosphite TPP into the blended liquid, ultrasonicate for 1 to 2 hours, and stir for 1 to 2 days under a nitrogen atmosphere at room temperature to obtain a side chain crosslinked sulfonated polyarylethersulfoneketone polymer.
[0020] Furthermore, in the step 1, the carboxyl-containing bisphenol monomer is 4-carboxyphenylhydroquinone, phenolphthalein or 4,4-bis(4-hydroxyphenyl)valeric acid, the dihalogen monomer is 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorobenzophenone, the sulfonic acid-containing bisphenol monomer is 4-sulfonic acid phenylhydroquinone, 2,5-dihydroxy-(1,1'-biphenyl)-4-sulfonic acid or potassium 2,5-dihydroxybenzenesulfonate, and the molar ratio of the carboxyl-containing bisphenol monomer, the dihalogen monomer and the sulfonic acid-containing bisphenol monomer is x:(x+y):y.
[0021] Furthermore, in the step 1, the molar ratio of the carboxyl-containing bisphenol monomer, the organic solvent, the water-carrying agent and the salt-forming agent is 0.1-0.9:2-8:2-8:2-5.
[0022] Furthermore, in the step 2, the mass ratio of the crosslinking agent Z, the catalyst TPP and the carboxyl-containing sulfonated polyarylethersulfoneketone is 0.03-0.12:0.01-0.04:1.
[0023] Furthermore, in the step 2, the mass ratio of the carboxyl-containing sulfonated poly(aryl ether sulfone ketone) to the organic solvent is 1:5-20.
[0024] Furthermore, the water-carrying agent is toluene or benzene; the salt-forming agent is anhydrous potassium carbonate or anhydrous sodium carbonate; the organic solvent in step one is one or a mixture of two or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide, and the organic solvent in step two is dimethylacetamide.
[0025] The side chain cross-linked sulfonated poly(aryl ether sulfone ketone) polymer prepared by the above method is used for preparing a cross-linked proton exchange membrane, specifically: the side chain cross-linked sulfonated poly(aryl ether sulfone ketone) polymer is used as a casting liquid, the casting liquid is naturally flattened on a clean glass plate, and the temperature is programmed to rise in a vacuum oven within a temperature range of 60 to 200° C., and then a cross-linked sulfonated poly(aryl ether sulfone ketone) proton exchange membrane is obtained.
[0026] Furthermore, the cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane is used in fuel cells.
[0027] Beneficial effects of the present invention: The present invention provides a chemically cross-linked proton exchange membrane based on carboxyl-containing sulfonated polyarylethersulfoneketone and Z for fuel cells, wherein the mass ratio of the above-mentioned Z to the carboxyl-containing sulfonated polyarylethersulfoneketone is 0.03-0.12:1, triphenyl phosphite (TPP) is used as a catalyst, and Z is introduced into the main chain of the sulfonated polyarylethersulfoneketone by amidation reaction between amino and carboxyl groups, and a cross-linked network is formed inside the sulfonated polyarylethersulfoneketone, so that the molecular chains become closer, and the heat resistance and dimensional stability are improved. In addition, the main chain and cross-linking bonds of the cross-linked membrane contain sulfonic acid groups at the same time, and the high sulfonic acid group content can improve the proton conductivity of the membrane. The test results show that the conductivity of the side chain cross-linked sulfonated polyarylethersulfoneketone proton exchange membrane of the present invention is 0.0678S cm at 80°C. -1 -0.0732S cm -1 . BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the infrared spectrum of the carboxyl-containing sulfonated poly(aryl ether sulfone ketone) and the side chain cross-linked sulfonated poly(aryl ether sulfone ketone) proton exchange membrane.
[0029] Figure 2 It is a bar graph showing the proton conductivity of the cross-linked membrane prepared in Example 1 as a function of temperature.
[0030] Figure 3 It is a bar graph showing the proton conductivity of the cross-linked membrane prepared in Example 2 as a function of temperature.
[0031] Figure 4It is a bar graph showing the proton conductivity of the cross-linked membrane prepared in Example 3 as a function of temperature.
[0032] Figure 5 It is a bar graph showing the proton conductivity of the cross-linked membrane prepared in Example 4 as a function of temperature.
[0033] Figure 6 This is a bar graph showing the proton conductivity of the cross-linked membrane prepared in Example 5 as a function of temperature.
[0034] Figure 7 It is a bar graph showing the proton conductivity of the cross-linked membrane prepared in Example 6 as a function of temperature.
[0035] Figure 8 It is a bar graph showing the proton conductivity of the cross-linked membrane prepared in Example 7 as a function of temperature.
[0036] Fig. 9 It is a bar graph showing the proton conductivity of the cross-linked membrane prepared in Example 8 as a function of temperature.
[0037] Fig.10 It is a bar graph showing the proton conductivity of the cross-linked membrane prepared in Example 9 as a function of temperature.
[0038] from Figures 2 to 10 It can be seen that with the increase of the mass fraction of the cross-linking agent Z, the proton conductivity shows a trend of first decreasing and then increasing. When the content of the cross-linking agent Z is higher than 10%wt, the cross-linked membrane exhibits a higher proton conductivity than pure carboxyl-containing sulfonated poly(arylethersulfoneketone) (SPPESA-COOH).
[0039] The present invention is described in detail below in conjunction with specific implementations and drawings. The scope of the present invention is not limited to this embodiment, but is defined by the scope of the claims. DETAILED DESCRIPTION
[0040] Hereinafter, the present invention will be described in further detail with reference to examples, which are for illustrative purposes only and should not be construed as limiting the scope of the present invention.
[0041] Example 1
[0042] A method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for a fuel cell, comprising the following steps:
[0043] (1) Under nitrogen protection, 0.4 mol of 4-carboxyphenylhydroquinone monomer, 1.0 mol of the sum of 4,4'-difluorobenzophenone and 4,4'-dichlorodiphenyl sulfone, and 0.6 mol of potassium 2,5-dihydroxybenzenesulfonate were weighed and added to a four-necked flask in sequence, and then 200 ml of an organic solvent, 315 ml of a water-carrying agent, and 250 g of a salt-forming agent were added to the four-necked flask. The water-carrying agent was allowed to carry water at 130° C. for 4 hours, and then the water-carrying agent was discharged, and the temperature was slowly raised to 190° C. After reacting for 24 hours, a carboxyl-containing sulfonated polyarylethersulfoneketone was obtained, wherein the water-carrying agent was toluene and the salt-forming agent was K 2 CO 3 , the solvent is dimethyl sulfoxide.
[0044] (2) Weigh 2 g of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) into a flask, add 20 ml of DMAc, and stir at room temperature for 12 h to form a uniform solution.
[0045] (3) Solid powder Z and 0.06 ml of triphenyl phosphite were added to the uniform solution in (2), and ultrasonicated for 2 h. The mixture was stirred for 36 h under a nitrogen atmosphere at room temperature to obtain a uniform casting solution, wherein the mass ratios of Z to sulfonated poly(aryl ether sulfone ketone) were 0.05:1, 0.07:1, 0.1:1, and 0.12:1, respectively.
[0046] (4) The casting solution obtained in (3) was poured onto a clean glass plate and naturally flattened, and then dried in an oven under a programmed temperature increase mode of 60, 80, 100, 120, 140, 160, 180 and 200°C (2 h each time).
[0047] (5) After natural cooling, the membrane is removed in deionized water and acidified in a sulfuric acid solution for 24 hours, followed by multiple rinses to remove the residual acid on the membrane, thereby finally obtaining a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for fuel cells.
[0048] The obtained side chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane was tested at 80°C, and the highest conductivity was 0.0718S cm -1 .
[0049] Example 2
[0050] A method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for a fuel cell, comprising the following steps:
[0051] (1) Under nitrogen protection, 0.4 mol of carboxyl-containing phenolphthalein monomer, 1.0 mol of the sum of 4,4'-difluorobenzophenone and 4,4'-dichlorodiphenyl sulfone, and 0.6 mol of potassium 2,5-dihydroxybenzenesulfonate are weighed and added to a four-necked flask in sequence, and then 260 ml of an organic solvent, 245 ml of a water-carrying agent, and 200 g of a salt-forming agent are added to the four-necked flask. The water-carrying agent is heated at 140° C. for 5 hours, and then the water-carrying agent is discharged, and the temperature is slowly raised to 180° C. After reacting for 24 hours, a carboxyl-containing sulfonated polyarylethersulfoneketone is obtained, wherein the water-carrying agent is benzene and the salt-forming agent is Na 2 CO 3 , the solvent is N-methylpyrrolidone.
[0052] (2) Weigh 2 g of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) into a flask, add 20 ml of DMAc, and stir at room temperature for 12 h to form a uniform solution.
[0053] (3) Add solid powder Z and 0.065 ml of triphenyl phosphite to the uniform solution in (2), and ultrasonicate for 2 hours. Stir for 36 hours under nitrogen atmosphere at room temperature to obtain a uniform casting solution, wherein the mass ratios of Z to sulfonated poly(arylethersulfoneketone) are 0.05:1, 0.07:1, 0.1:1, and 0.12:1, respectively.
[0054] (4) The casting solution obtained in (3) was poured onto a clean glass plate and naturally flattened, and then dried in an oven under a programmed temperature increase mode of 60, 80, 100, 120, 140, 160, 180 and 200°C (2 h each time).
[0055] (5) After natural cooling, the membrane is removed in deionized water and acidified in a sulfuric acid solution for 24 hours, followed by multiple rinses to remove the residual acid on the membrane, thereby finally obtaining a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for fuel cells.
[0056] The obtained side chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane was tested at 80 °C, and the highest conductivity was 0.0724 S cm -1 .
[0057] Example 3
[0058] A method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for a fuel cell, comprising the following steps:
[0059] (1) Under nitrogen protection, 0.4 mol of carboxyl-containing 4,4-bis(4-hydroxyphenyl)valeric acid monomer, 1.0 mol of the sum of 4,4'-difluorobenzophenone and 4,4'-dichlorodiphenyl sulfone, and 0.6 mol of potassium 2,5-dihydroxybenzenesulfonate were weighed and added to a four-necked flask in sequence, and then 200 ml of an organic solvent, 240 ml of a water-carrying agent, and 195 g of a salt-forming agent were added to the four-necked flask. The water-carrying agent was allowed to carry water at 140° C. for 4 hours, and then the water-carrying agent was discharged, and the temperature was slowly raised to 180° C. After reacting for 24 hours, a carboxyl-containing sulfonated polyarylethersulfoneketone was obtained, wherein the water-carrying agent was benzene and the salt-forming agent was Na 2 CO 3 , the solvent is dimethyl sulfoxide.
[0060] (2) Weigh 2 g of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) into a flask, add 20 ml of DMAc, and stir at room temperature for 12 h to form a uniform solution.
[0061] (3) Solid powder Z and 0.062 ml of triphenyl phosphite were added to the uniform solution in (2), and ultrasonicated for 2 h. The mixture was stirred for 36 h under nitrogen atmosphere at room temperature to obtain a uniform casting solution, wherein the mass ratios of Z to sulfonated poly(arylethersulfoneketone) were 0.05:1, 0.07:1, 0.1:1, and 0.12:1, respectively.
[0062] (4) The casting solution obtained in (3) was poured onto a clean glass plate and naturally flattened, and then dried in an oven under a programmed temperature increase mode of 60, 80, 100, 120, 140, 160, 180 and 200°C (2 h each time).
[0063] (5) After natural cooling, the membrane is removed in deionized water and acidified in a sulfuric acid solution for 24 hours, followed by multiple rinses to remove the residual acid on the membrane, thereby finally obtaining a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for fuel cells.
[0064] The obtained side chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane was tested at 80 °C, and the highest conductivity was 0.0719 S cm -1 .
[0065] Example 4
[0066] A method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for a fuel cell, comprising the following steps:
[0067] (1) Under nitrogen protection, 0.4 mol of 4-carboxyphenyl hydroquinone monomer, 1.0 mol of the sum of 4,4'-difluorobenzophenone and 4,4'-dichlorodiphenyl sulfone, and 0.6 mol of 4-sulfonic acid phenyl hydroquinone were weighed and added to a four-necked flask in sequence, and then 220 ml of organic solvent, 300 ml of water-carrying agent and 245 g of salt-forming agent were added to the four-necked flask. The water-carrying agent was allowed to carry water at 140° C. for 4 hours, and then the water-carrying agent was discharged, and the temperature was slowly raised to 190° C. After reacting for 24 hours, a carboxyl-containing sulfonated polyarylethersulfoneketone was obtained, wherein the water-carrying agent was toluene and the salt-forming agent was K 2 CO 3 , the solvent is N,N-dimethylformamide.
[0068] (2) Weigh 2 g of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) into a flask, add 20 ml of DMAc, and stir at room temperature for 12 h to form a uniform solution.
[0069] (3) Solid powder Z and 0.063 ml of triphenyl phosphite were added to the uniform solution in (2), and ultrasonicated for 2 h. The mixture was stirred for 36 h under a nitrogen atmosphere at room temperature to obtain a uniform casting solution, wherein the mass ratios of Z to sulfonated poly(arylethersulfoneketone) were 0.05:1, 0.07:1, 0.1:1, and 0.12:1, respectively.
[0070] (4) The casting solution obtained in (3) was poured onto a clean glass plate and naturally flattened, and then dried in an oven under a programmed temperature increase mode of 60, 80, 100, 120, 140, 160, 180 and 200°C (2 h each time).
[0071] (5) After natural cooling, the membrane is removed in deionized water and acidified in a sulfuric acid solution for 24 hours, followed by multiple rinses to remove the residual acid on the membrane, thereby finally obtaining a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for fuel cells.
[0072] The obtained side chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane was tested at 80 °C, and the highest conductivity was 0.0724 S cm -1 .
[0073] Example 5
[0074] A method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for a fuel cell, comprising the following steps:
[0075] (1) Under nitrogen protection, 0.4 mol of carboxyl-containing phenolphthalein monomer, 1.0 mol of the sum of 4,4'-difluorobenzophenone and 4,4'-dichlorodiphenyl sulfone, and 0.6 mol of 4-sulfonic acid phenyl hydroquinone are weighed and added to a four-necked flask in sequence, and then 255 ml of an organic solvent, 305 ml of a water-carrying agent, and 240 g of a salt-forming agent are added to the four-necked flask. The water-carrying agent is allowed to carry water at 120° C. for 4 hours, and then the water-carrying agent is discharged, and the temperature is slowly raised to 170° C. After reacting for 24 hours, a carboxyl-containing sulfonated polyarylethersulfoneketone is obtained, wherein the water-carrying agent is toluene and the salt-forming agent is K 2 CO 3 , the solvent is N,N-dimethylacetamide.
[0076] (2) Weigh 2 g of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) into a flask, add 20 ml of DMAc, and stir at room temperature for 12 h to form a uniform solution.
[0077] (3) Solid powder Z and 0.062 ml of triphenyl phosphite were added to the uniform solution in (2), and ultrasonicated for 2 h. The mixture was stirred for 36 h under nitrogen atmosphere at room temperature to obtain a uniform casting solution, wherein the mass ratios of Z to sulfonated poly(arylethersulfoneketone) were 0.05:1, 0.07:1, 0.1:1, and 0.12:1, respectively.
[0078] (4) The casting solution obtained in (3) was poured onto a clean glass plate and naturally flattened, and then dried in an oven under a programmed temperature increase mode of 60, 80, 100, 120, 140, 160, 180 and 200°C (2 h each time).
[0079] (5) After natural cooling, the membrane is removed in deionized water and acidified in a sulfuric acid solution for 24 hours, followed by multiple rinses to remove the residual acid on the membrane, thereby finally obtaining a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for fuel cells.
[0080] The obtained side chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane was tested at 80 °C, and the highest conductivity was 0.0729 S cm -1 .
[0081] Example 6
[0082] A method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for a fuel cell, comprising the following steps:
[0083] (1) Under nitrogen protection, 0.4 mol of carboxyl-containing 4,4-bis(4-hydroxyphenyl)valeric acid monomer, 1.0 mol of the sum of 4,4'-difluorobenzophenone and 4,4'-dichlorodiphenyl sulfone, and 0.6 mol of 4-sulfonic acid phenyl hydroquinone were weighed and added to a four-necked flask in sequence, and then 270 ml of an organic solvent, 240 ml of a water-carrying agent, and 235 g of a salt-forming agent were added to the four-necked flask. The water-carrying agent was allowed to carry water at 140° C. for 4 hours, and then the water-carrying agent was discharged, and the temperature was slowly raised to 190° C. After reacting for 24 hours, a carboxyl-containing sulfonated polyarylethersulfoneketone was obtained, wherein the water-carrying agent was benzene and the salt-forming agent was K 2 CO 3 , the solvent is N-methylpyrrolidone.
[0084] (2) Weigh 2 g of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) into a flask, add 20 ml of DMAc, and stir at room temperature for 12 h to form a uniform solution.
[0085] (3) Solid powder Z and 0.064 ml of triphenyl phosphite were added to the uniform solution in (2), and ultrasonicated for 2 h. The mixture was stirred for 36 h under a nitrogen atmosphere at room temperature to obtain a uniform casting solution, wherein the mass ratios of Z to sulfonated poly(arylethersulfoneketone) were 0.05:1, 0.07:1, 0.1:1, and 0.12:1, respectively.
[0086] (4) The casting solution obtained in (3) was poured onto a clean glass plate and naturally flattened, and then dried in an oven under a programmed temperature increase mode of 60, 80, 100, 120, 140, 160, 180 and 200°C (2 h each time).
[0087] (5) After natural cooling, the membrane is removed in deionized water and acidified in a sulfuric acid solution for 24 hours, followed by multiple rinses to remove the residual acid on the membrane, thereby finally obtaining a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for fuel cells.
[0088] The obtained side chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane was tested at 80 °C, and the highest conductivity was 0.0719 S cm -1 .
[0089] Example 7
[0090] A method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for a fuel cell, comprising the following steps:
[0091] (1) Under nitrogen protection, 0.4 mol of 4-carboxyphenylhydroquinone monomer, 1.0 mol of the sum of 4,4'-difluorobenzophenone and 4,4'-dichlorodiphenyl sulfone, and 0.6 mol of 2,5-dihydroxy-(1,1'-biphenyl)-4-sulfonic acid were weighed and added to a four-necked flask in sequence, and then 195 ml of an organic solvent, 300 ml of a water-carrying agent, and 190 g of a salt-forming agent were added to the four-necked flask. The water-carrying agent was allowed to carry water at 130° C. for 4 hours, and then the water-carrying agent was discharged, and the temperature was slowly raised to 190° C. After reacting for 24 hours, a carboxyl-containing sulfonated polyarylethersulfoneketone was obtained, wherein the water-carrying agent was toluene and the salt-forming agent was Na 2 CO 3 , the solvent is dimethyl sulfoxide.
[0092] (2) Weigh 2 g of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) into a flask, add 20 ml of DMAc, and stir at room temperature for 12 h to form a uniform solution.
[0093] (3) Add solid powder Z and 0.065 ml of triphenyl phosphite to the uniform solution in (2), and ultrasonicate for 2 hours. Stir for 36 hours under nitrogen atmosphere at room temperature to obtain a uniform casting solution, wherein the mass ratios of Z to sulfonated poly(arylethersulfoneketone) are 0.05:1, 0.07:1, 0.1:1, and 0.12:1, respectively.
[0094] (4) The casting solution obtained in (3) was poured onto a clean glass plate and naturally flattened, and then dried in an oven under a programmed temperature increase mode of 60, 80, 100, 120, 140, 160, 180 and 200°C (2 h each time).
[0095] (5) After natural cooling, the membrane is removed in deionized water and acidified in a sulfuric acid solution for 24 hours, followed by multiple rinses to remove the residual acid on the membrane, thereby finally obtaining a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for fuel cells.
[0096] The obtained side chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane was tested at 80 °C, and the highest conductivity was 0.0725 S cm -1 .
[0097] Example 8
[0098] A method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for a fuel cell, comprising the following steps:
[0099] (1) Under nitrogen protection, 0.4 mol of carboxyl-containing phenolphthalein monomer, 1.0 mol of the sum of 4,4'-difluorobenzophenone and 4,4'-dichlorodiphenyl sulfone, and 0.6 mol of 2,5-dihydroxy-(1,1'-biphenyl)-4-sulfonic acid were weighed and added to a four-necked flask in sequence, and then 195 ml of an organic solvent, 290 ml of a water-carrying agent, and 230 g of a salt-forming agent were added to the four-necked flask. The water-carrying agent was allowed to carry water at 140° C. for 4 hours, and then the water-carrying agent was discharged, and the temperature was slowly raised to 180° C. After reacting for 24 hours, a carboxyl-containing sulfonated polyarylethersulfoneketone was obtained, wherein the water-carrying agent was toluene and the salt-forming agent was K 2 CO 3 , the solvent is dimethyl sulfoxide.
[0100] (2) Weigh 2 g of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) into a flask, add 20 ml of DMAc, and stir at room temperature for 12 h to form a uniform solution.
[0101] (3) Solid powder Z and 0.06 ml of triphenyl phosphite were added to the uniform solution in (2), and ultrasonicated for 2 h. The mixture was stirred for 36 h under a nitrogen atmosphere at room temperature to obtain a uniform casting solution, wherein the mass ratios of Z to sulfonated poly(arylethersulfoneketone) were 0.05:1, 0.07:1, 0.1:1, and 0.12:1, respectively.
[0102] (4) The casting solution obtained in (3) was poured onto a clean glass plate and naturally flattened, and then dried in an oven under a programmed temperature increase mode of 60, 80, 100, 120, 140, 160, 180 and 200°C (2 h each time).
[0103] (5) After natural cooling, the membrane is removed in deionized water and acidified in a sulfuric acid solution for 24 hours, followed by multiple rinses to remove the residual acid on the membrane, thereby finally obtaining a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for fuel cells.
[0104] The obtained side chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane was tested at 80 °C, and the highest conductivity was 0.0728 S cm -1 .
[0105] Example 9
[0106] A method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for a fuel cell, comprising the following steps:
[0107] (1) Under nitrogen protection, 0.4 mol of carboxyl-containing 4,4-bis(4-hydroxyphenyl)valeric acid monomer, 1.0 mol of the sum of 4,4'-difluorobenzophenone and 4,4'-dichlorodiphenyl sulfone, and 0.6 mol of 2,5-dihydroxy-(1,1'-biphenyl)-4-sulfonic acid were weighed and added to a four-necked flask in sequence, and then 240 ml of an organic solvent, 300 ml of a water-carrying agent, and 230 g of a salt-forming agent were added to the four-necked flask. The water-carrying agent was allowed to carry water at 140° C. for 4 hours, and then the water-carrying agent was discharged, and the temperature was slowly raised to 190° C. After reacting for 24 hours, a carboxyl-containing sulfonated polyarylethersulfoneketone was obtained, wherein the water-carrying agent was toluene and the salt-forming agent was K 2 CO 3 , the solvent is N,N-dimethylacetamide.
[0108] (2) Weigh 2 g of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) into a flask, add 20 ml of DMAc, and stir at room temperature for 12 h to form a uniform solution.
[0109] (3) Add solid powder Z and 0.065 ml of triphenyl phosphite to the uniform solution in (2), and ultrasonicate for 2 hours. Stir for 36 hours under nitrogen atmosphere at room temperature to obtain a uniform casting solution, wherein the mass ratios of Z to sulfonated poly(arylethersulfoneketone) are 0.05:1, 0.07:1, 0.1:1, and 0.12:1, respectively.
[0110] (4) The casting solution obtained in (3) was poured onto a clean glass plate and naturally flattened, and then dried in an oven under a programmed temperature increase mode of 60, 80, 100, 120, 140, 160, 180 and 200°C (2 h each time).
[0111] (5) After natural cooling, the membrane is removed in deionized water and acidified in a sulfuric acid solution for 24 hours, followed by multiple rinses to remove the residual acid on the membrane, thereby finally obtaining a side-chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane for fuel cells.
[0112] The obtained side chain cross-linked sulfonated poly(arylethersulfoneketone) proton exchange membrane was tested at 80 °C, and the highest conductivity was 0.0732 S cm -1 .
Claims
1. A method for preparing a side chain cross-linked sulfonated polyarylethersulfoneketone polymer, characterized in that: The carboxyl-containing sulfonated polyarylethersulfoneketone undergoes an amidation reaction with the crosslinking agent Z under the action of a catalyst, and the reaction chemical formula is as follows: Wherein, x=0.1~0.9, y=0.1~0.9; Ar1 is: Ar2 is: Ar3 is: The crosslinking agent Z is: The catalyst is triphenyl phosphite TPP; the mass ratio of the crosslinking agent Z to the carboxyl-containing sulfonated polyarylethersulfoneketone is 0.1-0.12:
1.
2. The method for preparing a side chain cross-linked sulfonated polyarylethersulfoneketone polymer according to claim 1, characterized in that: The specific steps are as follows: Step 1: Preparation of carboxyl-containing sulfonated poly(aryl ether sulfone ketone) Under the protection of inert gas, a carboxyl-containing bisphenol monomer, a dihalogen monomer and a sulfonic acid-containing bisphenol monomer are mixed, and then an organic solvent, a water-carrying agent and a salt-forming agent are added, and the water-carrying agent carries water at 120-140° C. for 3-6 hours, and then the water-carrying agent is discharged, and the temperature is slowly raised to 170-190° C., and the reaction is carried out for 15-30 hours to obtain a carboxyl-containing sulfonated polyarylethersulfoneketone; Step 2: Add the carboxyl-containing sulfonated polyarylethersulfoneketone obtained in step 1 and the crosslinking agent Z to an organic solvent to obtain a blended liquid, dropwise add the catalyst triphenyl phosphite TPP into the blended liquid, ultrasonicate for 1 to 2 hours, and stir for 1 to 2 days under a nitrogen atmosphere at room temperature to obtain a side chain crosslinked sulfonated polyarylethersulfoneketone polymer.
3. The method for preparing a side chain cross-linked sulfonated polyarylethersulfoneketone polymer according to claim 2, characterized in that: In the step 1, the carboxyl-containing bisphenol monomer is 4-carboxylphenylhydroquinone, phenolphthalein or 4,4-bis(4-hydroxyphenyl)valeric acid, the dihalogen monomer is 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorobenzophenone, the sulfonic acid-containing bisphenol monomer is 4-sulfonic acid phenylhydroquinone, 2,5-dihydroxy-(1,1'-biphenyl)-4-sulfonic acid or potassium 2,5-dihydroxybenzenesulfonate, and the molar ratio of the carboxyl-containing bisphenol monomer, the dihalogen monomer and the sulfonic acid-containing bisphenol monomer is x:(x+y):y.
4. The method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) polymer according to claim 2, characterized in that: In the step 1, the carboxyl-containing bisphenol monomer, the organic solvent, the water-carrying agent and the salt-forming agent are added in a molar ratio of 0.1-0.9:2-8:2-8:2-5.
5. The method for preparing a side chain cross-linked sulfonated polyarylethersulfoneketone polymer according to claim 2, characterized in that: In the step 2, the mass ratio of the crosslinking agent Z, the catalyst TPP and the carboxyl-containing sulfonated polyarylethersulfoneketone is 0.1-0.12:0.01-0.04:
1.
6. The method for preparing a side chain cross-linked sulfonated poly(arylethersulfoneketone) polymer according to claim 2, characterized in that: In the step 2, the mass ratio of the carboxyl-containing sulfonated poly(aryl ether sulfone ketone) to the organic solvent is 1:5-20.
7. The method for preparing a side-chain cross-linked sulfonated poly(arylethersulfoneketone) polymer according to claim 2, characterized in that: The water-carrying agent is toluene or benzene; the salt-forming agent is anhydrous potassium carbonate or anhydrous sodium carbonate; the organic solvent in step one is one or a mixture of two or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide, and the organic solvent in step two is dimethylacetamide.
8. Use of a side chain cross-linked sulfonated poly(aryl ether sulfone ketone) polymer prepared by the method for preparing a side chain cross-linked sulfonated poly(aryl ether sulfone ketone) polymer according to any one of claims 1 to 7, characterized in that: The side chain cross-linked sulfonated polyarylethersulfoneketone polymer is used to prepare a cross-linked proton exchange membrane, specifically: the side chain cross-linked sulfonated polyarylethersulfoneketone polymer is used as a casting liquid, the casting liquid is naturally flattened on a clean glass plate, and the temperature is programmed to rise in a vacuum oven within a temperature range of 60 to 200° C., and then a cross-linked sulfonated polyarylethersulfoneketone proton exchange membrane is obtained.
9. The use according to claim 8, characterized in that: The cross-linked sulfonated polyarylethersulfoneketone proton exchange membrane is used for fuel cells.
Citation Information
Patent Citations
Polyarylether nitrile / epoxy resin copolymerized modified composition and preparation method and application thereof
CN104045978A
Arylene ether nitrile proton exchange membrane including side chain with flexible sulfonic acid ion cluster structure and preparation method thereof
CN106084208A