Copper alloy with high-density twins and low mismatch precipitation phase and preparation method thereof

By optimizing the element ratio and process treatment, a copper alloy with high density nanotwins and low mismatch precipitated phases was prepared, which solved the problem of comprehensive performance degradation of copper alloy materials in terms of strength, conductivity and extensibility, and achieved resistance to Significant improvement in tensile strength, electrical conductivity and elongation.

CN116240423BActive Publication Date: 2024-10-08HENAN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310147414.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-10-08
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

Existing copper alloy materials have problems with comprehensive performance decline in improving strength, conductivity and elongation. In particular, the high mismatch between the precipitated phase and the matrix interface causes the material to easily break and reduce elongation.

Method used

Using a method that combines element ratio optimization, grain refinement process and controlled heat treatment process, a copper alloy with high density nanotwins and low mismatch precipitate phase is prepared. Through high-temperature vacuum melting, hot extrusion, and solid solution treatment , low-temperature dynamic plastic deformation and short-term aging treatment to form a copper alloy with excellent properties.

Benefits of technology

It achieves the simultaneous improvement of the tensile strength, electrical conductivity and elongation of the copper alloy, has high comprehensive performance, avoids the problems of element segregation and performance degradation, has low cost and simple process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116240423B_ABST
    Figure CN116240423B_ABST
Patent Text Reader

Abstract

A copper alloy with high-density twins and low mismatch precipitation phases, including the following components in mass percentage: 1.0-1.5% Ni, 0.7-1.2% Co, 0.45-0.65% Si, and the remainder is copper; the copper alloy contains 25-35% volume of high-density nano-scale twins, and the copper alloy is also uniformly distributed with a nano-scale precipitation phase with a particle size of 2-5 nm, and the precipitation phase and the copper matrix interface have a mismatch of 0.5-0.75%. The copper alloy prepared by the present invention, by optimizing the proportioning relationship of the four elements in the alloy, fully and comprehensively plays the advantages of the four materials of copper, nickel, cobalt and silicon, avoids the occurrence of the problems such as element segregation in the finished copper alloy material, and makes high-density nano-twins and low mismatch precipitation phases exist in the alloy matrix at the same time, so that the tensile strength, electrical conductivity and elongation of the finished copper alloy are significantly improved synchronously, with excellent comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper alloy preparation, in particular to the preparation of a high-performance copper alloy material with high strength, high conductivity and high elongation and having high-density twins and low mismatch precipitation phases. Background Art

[0002] Copper-based alloys have become the most widely used alloys in the electronics and electrical industry due to their excellent strength, conductivity, corrosion resistance and other excellent properties. However, with the rapid development of the electronics and electrical industry, higher requirements have been placed on the material properties of copper alloys.

[0003] At present, the existing technology mainly improves the performance of copper alloys in two ways: one is the trace element strengthening method, that is, by adding solid solution elements, precipitation strengthening elements, etc. to improve the precipitation phase and organization inside the alloy, so as to improve the strength and other properties of the material. The addition of trace elements is the best way to optimize material properties and improve material defects, but this method will cause element loss and segregation during the smelting process, and the element ratio range is sensitive to the performance. The second method is the organizational structure strengthening method, that is, the original coarse grains of the material are refined to ultrafine grains of about 100 nm through a process. This method includes equal-diameter angular extrusion, high-pressure torsion, etc. This method can double the strength of the material, but the reduction of other properties such as conductivity and elongation is also obvious, resulting in a decrease in overall performance.

[0004] For precipitation-strengthened copper alloys, the state of the precipitate phase affects the performance of the material, and the precipitation of the precipitate phase is usually used to improve the strength, conductivity and other properties of the material. However, there is a large mismatch between the precipitate phase and the matrix interface, which causes dislocations to accumulate near the precipitate phase, making the material easy to break and the elongation significantly reduced.

[0005] Nano twins have the advantages of high strength, good plasticity and work hardening. Compared with traditional precipitation strengthening and grain refinement, which usually produce high strain gradients around them and cause stress concentration problems, there is almost no strain / stress concentration around nano twin grains under uniform plastic strain, so nano twins can effectively improve the strength and ductility of materials. However, twin structures are usually not easy to appear in high dislocation energy materials such as copper alloys, because there are many slip systems that can be activated inside copper alloy materials, and dislocation slip often replaces the generation of twins.

[0006] Therefore, how to effectively improve the internal structure of copper alloys so that their strength, plasticity, conductivity, ductility and other properties can be significantly improved simultaneously, so as to prepare copper-based alloys with significantly improved comprehensive properties, is an urgent problem to be solved by technical personnel in this field. Summary of the invention

[0007] The technical purpose of the present invention is to provide a new method for preparing copper alloys by combining element ratio optimization, grain refinement process and controlled heat treatment process, so that high-density nano twins and low mismatch precipitation phases exist in the alloy matrix at the same time, so that the tensile strength, conductivity and elongation of the finished copper alloy are significantly improved simultaneously, and it has excellent comprehensive performance.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is: a copper alloy with high-density twins and low mismatch precipitation phases, comprising the following components in mass percentage: 1.0-1.5% Ni, 0.7-1.2% Co, 0.45-0.65% Si, and the remainder is copper and unavoidable impurity elements; the copper alloy contains 25-35% volume of high-density nanoscale twins, and the copper alloy is also uniformly distributed with nanoscale precipitation phases with a particle size of 2-5 nm, and the interface between the precipitation phase and the copper matrix has a mismatch of 0.5-0.75%.

[0009] Preferably, the mass ratio of (Ni+Co) / Si in the copper alloy is 4-4.5.

[0010] A method for preparing a copper alloy having high-density twins and low mismatch precipitation phases comprises the following steps:

[0011] Step 1: Alloy smelting

[0012] According to the above mass percentage ratio, nickel, cobalt, silicon and copper are weighed respectively and placed in a high-frequency vacuum melting furnace, and are subjected to high-temperature vacuum melting under inert gas protection conditions, and then cast at 900-1100° C., and air-cooled to room temperature to obtain alloy ingots for standby use;

[0013] Step 2: Hot extrusion

[0014] The alloy ingot obtained in step 1 is heated to 900-1050°C for heat preservation for 2-3 hours, and then hot-extruded into a rod blank for standby use;

[0015] Step 3: Solution treatment

[0016] Under inert gas protection conditions, the rod blank obtained in step 2 is subjected to a heat preservation solid solution treatment in an environment of 900-960° C. for 1.5-2 hours, and then water quenched;

[0017] Step 4: Twinning Preparation

[0018] The billet after water quenching in step 3 is subjected to multiple low-temperature dynamic plastic deformations at (-196)- (-150)℃ by dynamic plastic deformation equipment, so that the final deformation ε>1.9; where ε = ln (L0 / L f ), L0 is the initial height of the billet, L fis the final height of the billet after deformation;

[0019] Step 5: Introduce the precipitated phase

[0020] Under inert gas protection conditions, the sample prepared by twinning in step 4 is placed in a heating furnace at a temperature of 400-550° C. for heat preservation and aging treatment for 10-15 min. After cooling to room temperature, a finished copper alloy with high-density twins and low mismatch precipitation phase is obtained.

[0021] Preferably, in step 1, before the high-temperature vacuum melting, the high-frequency vacuum melting furnace needs to be evacuated to a pressure of 8×10 -2 - 6×10 -2 Pa, and then, inert gas is filled into the furnace to make the pressure in the furnace 0.03-0.05 MPa.

[0022] Preferably, the inert gas is argon.

[0023] Preferably, in step 1, the temperature during the high-temperature vacuum melting is 1000-1200°C.

[0024] Preferably, in step three, the heat preservation and solution treatment is carried out in a box-type resistance furnace.

[0025] Preferably, in step 4, during the low-temperature dynamic plastic deformation process, the rod blank needs to be cooled with liquid nitrogen for 3-5 minutes before each deformation.

[0026] Preferably, in step 4, the dynamic plastic deformation device is a Hopkinson pressure bar, and the strain rate of the dynamic plastic deformation device is greater than 10 -3 s -1 .

[0027] Preferably, in step five, the heating furnace is a vacuum tube furnace, and the cooling process is carried out in an air environment.

[0028] Beneficial effects of the present invention:

[0029] 1. The copper alloy with high-density twins and low mismatch precipitation phase prepared by the present invention fully and comprehensively utilizes the advantages of copper, nickel, cobalt and silicon by optimizing the ratio of the four elements Cu-Ni-Co-Si in the alloy, avoiding the occurrence of problems such as element segregation in the finished copper alloy material, and making high-density nano twins and low mismatch precipitation phases exist in the alloy matrix at the same time, so that the tensile strength, electrical conductivity and elongation of the finished copper alloy are significantly improved synchronously, and have excellent comprehensive performance. According to measurements, the tensile strength of the copper alloy with high-density twins and low mismatch precipitation phase prepared by the present invention reached more than 680Mpa, the electrical conductivity reached more than 37%IACS, and the elongation reached more than 10.4%, with excellent comprehensive performance and good application prospects.

[0030] 2. The high-performance copper alloy preparation process of the present invention adopts a low-temperature dynamic plastic deformation method to introduce high-density nanotwins into the copper alloy, so that the volume content of nanotwins in the finished copper alloy is >25%, and the grain size of the material is refined, thereby significantly improving the material strength; the introduction of high-density nanotwins maintains high elongation and conductivity while having high strength, so that the finished copper alloy has excellent comprehensive performance.

[0031] 3. The high-performance copper alloy preparation process of the present invention adopts a short-time precipitation method, so that high-density twins and precipitated phases in the copper alloy coexist, thereby further improving the strength, conductivity and elongation of the material.

[0032] 4. Compared with multi-stage aging treatment, the high-performance copper alloy preparation process of the present invention has simple steps, convenient operation, high efficiency and low cost in terms of aging treatment.

[0033] 5. The present invention selects copper-nickel-silicon alloy as raw material, optimizes the element ratio and adds cobalt element to integrate into the matrix and further improves the proportion of precipitation phase after high-temperature solution treatment. When the material is placed in a low-temperature and high-speed deformation state by low-temperature dynamic plastic deformation method, the interaction between the material grains and dislocations requires greater shear stress. At this time, the plastic deformation of the material is difficult to be carried out in a slip manner, so a large number of twins can be formed inside the material. At the same time, after low-temperature dynamic plastic deformation, a short-time heat treatment process is carried out. The shortening of the heat treatment time ensures that the twins will not be annihilated by the migration of grain boundaries, ensuring the high density of twins inside the material. In addition, after the supersaturated solid solution formed by solution treatment and after low-temperature dynamic plastic deformation, there are high-density defects and high energy storage in the organization, which can become a more effective nucleation point when the precipitation phase is precipitated. The use of short-time aging ensures high-density twins, and the optimization of the aging temperature ensures the low mismatch between the precipitation phase and the matrix. Therefore, the material of the present invention obtains excellent comprehensive performance.

[0034] 6. The high-performance copper alloy preparation process of the present invention limits the raw material ratio to the rule of (Ni+Co):Si atomic ratio of 2:1. This is to enable the alloy to form a sufficient and uniform precipitation phase (Ni,Co)2Si inside during preparation, so as to overcome the problem of insufficient precipitation caused by imprecise element control. In addition, in the twin preparation step, the material's dislocation energy is reduced through ultra-low temperature and high-speed deformation, and high-density twins that have not been previously introduced are introduced, thus overcoming the problem of the difficulty in preparing high-density twins in copper alloys. In the step of introducing the precipitation phase, an ultra-low mismatch precipitation phase is introduced by precisely controlling the aging time and temperature, and at the same time, the existence of high twins is guaranteed during the aging process. The combination of the two obtains high comprehensive performance that has not been previously achieved, thus overcoming the problem of the difficulty of coexistence of high-density twins and precipitation phases.

[0035] 7. The high-performance copper alloy preparation process of the present invention, the operation of keeping warm for 2-3 hours during the hot extrusion process can make the alloy ingot fully heated, and prevent the internal structural defects of the alloy caused by uneven heating of the alloy during the hot extrusion process. The high-temperature treatment environment of 900~960℃ in the solution treatment step can make the alloy elements fully dissolved into the matrix, so that the subsequent precipitation phase can precipitate continuously. The ultra-low temperature environment of -196 ~ -150℃ in the twin preparation step ensures that the twins can appear more fully under high-speed deformation conditions (that is, the twins can have a high volume fraction); the introduction of 400~550℃, 10~15 min short-time and efficient treatment in the precipitation phase step avoids the migration of the formed twins, ensures the high volume fraction of the twins in the aging process, and also makes the precipitation phase more uniform. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a microstructure morphology diagram of a high-density twinned copper alloy obtained in Example 1 of the present invention;

[0037] Figure 2 This is a microstructure morphology diagram of a high-performance copper alloy having a combination of high-density twins and nano-precipitated phases obtained in Example 2 of the present invention;

[0038] Figure 3 for Figure 2 Dark field microstructure morphology;

[0039] Figure 4 This is a mismatch image of the high-performance copper alloy precipitate phase and the matrix obtained in Example 2 of the present invention, which has a combination of high-density twins and nano-precipitates. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0041] A copper alloy with high-density twins and low-mismatch precipitation phases comprises the following components in mass percentage: 1.0-1.5% Ni, 0.7-1.2% Co, 0.45-0.65% Si, and the remainder is copper and unavoidable impurity elements; the copper alloy contains more than 25% volume of high-density nano-scale twins, and the nano-scale precipitation phases are uniformly distributed in the copper alloy.

[0042] The preparation method of the copper alloy having high-density twins and low mismatch precipitation phase specifically comprises the following steps:

[0043] (1) Alloy smelting: Pure copper is used as the matrix, and the reinforcing phases are pure nickel, pure cobalt, and pure silicon. In terms of mass percentage, the contents are Ni 1.0%~1.5%, Co 0.7%~1.2%, and Si 0.45%~0.65%, respectively. The material is melted in a high-temperature vacuum until the pressure in the furnace is 6×10 -2 Pa, inert gas is introduced for protection during the smelting process; the smelted alloy is heated to 900~1050℃, kept warm for 2 hours, and hot extruded into rods.

[0044] (2) Solution treatment: The rod blank is solution treated at 960℃ for 1h under the protection of inert gas.

[0045] (3) Twin preparation: The solution treated alloy was subjected to low temperature dynamic plastic deformation using a dynamic plastic deformation device. The deformation temperature was in a liquid nitrogen environment (-196°C). The final deformation amount ε>1.9, ε = ln (L0 / L f ), L0 is the initial height of the sample, L f It is the final height of the material after deformation.

[0046] (4) Introducing precipitated phase: The sample with introduced twins is placed in a heating furnace for aging treatment at a temperature of 400°C-550°C and an aging time of 15 min.

[0047] Furthermore, the mass ratio of (Ni+Co) / Si in step (1) is about 4.2.

[0048] Furthermore, in the dynamic plastic deformation process in step (3), the sample is cooled with liquid nitrogen for 3 minutes before each deformation.

[0049] Furthermore, the dynamic plastic deformation equipment for preparing the twins is a Hopkinson pressure bar.

[0050] Furthermore, in the dynamic plastic deformation process in step (3), the strain rate of the dynamic plastic deformation device is greater than 10 -3 s -1 .

[0051] Furthermore, the aging treatment process of the sample in step (4) is to place the sample at a set temperature before performing aging treatment on the sample.

[0052] The term "solution treatment" used in the present invention refers to the process in which the equilibrium transformation is suppressed during the solidification of the solid solution to obtain a metastable supersaturated solid solution single-phase structure. The term "aging treatment" used in the present invention refers to a heat treatment process in which a metal or alloy workpiece (such as low-carbon steel, etc.) is placed at a higher temperature or room temperature to maintain its shape and size after high-temperature quenching or a certain degree of cold working deformation, and the performance changes over time.

[0053] The process method of the present invention combines element ratio optimization with grain refinement technology, and its purpose is to make high-density nano twins and precipitated phases exist in the matrix at the same time, so that the strength, conductivity and elongation of the copper alloy are significantly improved simultaneously.

[0054] Example 1

[0055] In this embodiment, a copper alloy having only high-density twins is prepared. The copper alloy is composed of the following alloys in percentage by mass: 1.35% nickel, 1.0% cobalt, 0.55% silicon, and the remainder copper.

[0056] The specific preparation method of the copper alloy in this embodiment is as follows:

[0057] Step 1: Alloy smelting:

[0058] According to the above alloy ratio, pure nickel, pure cobalt, pure silicon, pure chromium and the prepared standard electrolytic copper with a purity of not less than 99% are weighed respectively, put into a high-frequency vacuum melting furnace for melting, and evacuate the furnace until the pressure inside is 6×10 -2 Pa, and then argon gas is injected to make the pressure in the furnace 0.03 MPa. Next, the temperature in the furnace is controlled at 1000-1200°C, and casting is carried out at 900-1100°C, and air-cooled to room temperature to form an alloy ingot for standby use;

[0059] Step 2, hot extrusion: heat the alloy ingot obtained in step 1 to 900-1050°C, keep it warm for 2 hours, and hot extrude it into a rod blank for standby use;

[0060] Step 3: Solution treatment: Place the rod blank obtained in step 2 into a box-type resistance furnace, add argon gas for protection, keep the temperature at 960°C for 1.5 hours, and quench with water.

[0061] Step 4: Twin preparation: The alloy after solution treatment is prepared for twin preparation. The alloy is subjected to low temperature dynamic plastic deformation using a Hopkinson bar. The deformation temperature is in a liquid nitrogen environment (-196°C). The final deformation amount ε = 2.0, ε = ln (L0 / L f ), L0 is the initial height of the sample, L f is the final height of the material after deformation. Each time the sample is deformed, it is immersed in liquid nitrogen temperature for 3 min to obtain a copper alloy with high-density twins.

[0062] The performance test of the finished copper alloy obtained in this embodiment is as follows:

[0063] The microstructure of the copper alloy with high-density twins prepared in this embodiment was observed using a transmission electron microscope. The results are shown in the attached figure. Figure 1 As shown. Figure 1 It can be clearly seen that there are a large number of high-density nano-scale twins evenly distributed in the copper alloy. The tensile strength of the finished copper alloy obtained in this embodiment is 736.2MPa, the conductivity is 24.5%IACS, and the elongation is 9.7%. (See Table 1 below).

[0064] Example 2

[0065] In this embodiment, a copper alloy with high-density twins and low mismatch precipitation phase is prepared. The copper alloy is composed of the following alloys in percentage by mass: 1.35% nickel, 1.0% cobalt, 0.55% silicon, and the balance is copper.

[0066] The specific preparation method of the high performance copper alloy in this embodiment is:

[0067] Step 1: Alloy smelting:

[0068] According to the above alloy ratio, pure nickel, pure cobalt, pure silicon, pure chromium and the prepared standard electrolytic copper with a purity of not less than 99% are weighed respectively, put into a high-frequency vacuum melting furnace for melting, and evacuate the furnace until the pressure inside is 6×10 -2 Pa, and then argon gas is injected to make the pressure in the furnace 0.03 MPa. Next, the temperature in the furnace is controlled at 1100°C, and casting is carried out at 1000°C, and air-cooled to room temperature to form an alloy ingot for standby use;

[0069] Step 2, hot extrusion: heat the alloy ingot obtained in step 1 to 1000°C, keep it warm for 2 hours, and hot extrude it into a rod blank for standby use;

[0070] Step 3: Solution treatment: Place the rod blank obtained in step 2 into a box-type resistance furnace, add argon gas for protection, keep the temperature at 960°C for 1.5 hours, and quench with water.

[0071] Step 4: Twin preparation: The alloy after the solution treatment is prepared for twin preparation. The alloy is subjected to low-temperature dynamic plastic deformation using a Hopkinson bar. The deformation temperature is in a liquid nitrogen environment (-196°C), and the final deformation amount ε = 2.0. Each time the deformation is performed, the sample is immersed in liquid nitrogen temperature for 3 min.

[0072] Step 5. Introduction of precipitate phase: The alloy after twin preparation is taken for introduction of precipitate phase. The alloy is aged in a vacuum tube furnace to introduce the precipitate phase. Argon gas is used for protection throughout the aging process. After the temperature in the furnace is controlled to rise to 450°C, the sample is placed in a vacuum tube furnace for insulation treatment for 15 minutes. The sample is then taken out and cooled to room temperature to obtain a high-performance copper alloy with high-density twins and precipitate phases.

[0073] The performance test of the finished copper alloy obtained in this embodiment is as follows:

[0074] The microstructure of the copper alloy with high-density twins prepared in this embodiment was observed using a transmission electron microscope. The results are shown in the attached figure. Figure 2 As shown. Figure 2 It can be seen that nano twins and nano-scale precipitation phases coexist in the finished copper alloy with high-density twins. Figure 3 for Figure 2 The dark field phase image shows the distribution of the precipitated phase. Figure 4 The mismatch image of the high-performance copper alloy precipitate phase and the matrix obtained in Example 2 of the present invention, which has a combination of high-density twins and nano-precipitates, is shown in FIG. Figure 4 It can be seen that the precipitated phase in the finished copper alloy has an ultra-low mismatch with the matrix. The tensile strength of the finished copper alloy obtained in this embodiment is tested to be 816.4 MPa, the conductivity is 40.2% IACS, and the elongation is 11.3%. (See Table 1 below).

[0075] Example 3

[0076] In this embodiment, a copper alloy with high-density twins and low mismatch precipitation phase is prepared. The copper alloy is composed of the following alloys in percentage by mass: 1.35% nickel, 1.0% cobalt, 0.55% silicon, and the balance is copper.

[0077] The specific preparation method of the high performance copper alloy in this embodiment is the same as that in Embodiment 2, except that the temperature of the aging treatment in the vacuum tube furnace in step 5 is adjusted to 400°C.

[0078] The performance test of the finished copper alloy obtained in this embodiment shows that its tensile strength is 760.5 MPa, the electrical conductivity is 37.4% IACS, and the elongation is 11.0%. (See Table 1 below).

[0079] Example 4

[0080] In this embodiment, a copper alloy with high-density twins and low mismatch precipitation phase is prepared. The copper alloy is composed of the following alloys in percentage by mass: 1.35% nickel, 1.0% cobalt, 0.55% silicon, and the balance is copper.

[0081] The specific preparation method of the high performance copper alloy in this embodiment is the same as that in Embodiment 2, except that the temperature of the aging treatment in the vacuum tube furnace in step 5 is adjusted to 500°C.

[0082] The performance test of the finished copper alloy obtained in this embodiment shows that its tensile strength is 772.5 MPa, the electrical conductivity is 42.3% IACS, and the elongation is 10.4%. (See Table 1 below).

[0083] Example 5

[0084] In this embodiment, a copper alloy with high-density twins and low mismatch precipitation phase is prepared. The copper alloy is composed of the following alloys in percentage by mass: 1.35% nickel, 1.0% cobalt, 0.55% silicon, and the balance is copper.

[0085] The specific preparation method of the high performance copper alloy in this embodiment is the same as that in Embodiment 2, except that the temperature of the aging treatment in the vacuum tube furnace in step 5 is adjusted to 550°C.

[0086] The performance test of the finished copper alloy obtained in this embodiment shows that its tensile strength is 680.7 MPa, the electrical conductivity is 43.9% IACS, and the elongation is 13.5%. (See Table 1 below).

[0087] Example 6

[0088] In this embodiment, a copper alloy with high-density twins and low mismatch precipitation phase is prepared. The copper alloy is composed of the following alloys in percentage by mass: 1% nickel, 1.2% cobalt, 0.45% silicon, and the balance is copper.

[0089] The specific preparation method of the high performance copper alloy in this embodiment is:

[0090] Step 1: Alloy smelting:

[0091] According to the above alloy ratio, pure nickel, pure cobalt, pure silicon, pure chromium and the prepared standard electrolytic copper with a purity of not less than 99% are weighed respectively, put into a high-frequency vacuum melting furnace for melting, and evacuate the furnace until the pressure inside is 6×10 -2Pa, and then argon gas is injected to make the pressure in the furnace 0.03 MPa. Next, the temperature in the furnace is controlled at 1200°C, and casting is carried out at 1100°C, and air-cooled to room temperature to form an alloy ingot for standby use;

[0092] Step 2, hot extrusion: heat the alloy ingot obtained in step 1 to 900°C, keep it warm for 2 hours, and hot extrude it into a rod blank for standby use;

[0093] Step 3: Solution treatment: Place the rod blank obtained in step 2 into a box-type resistance furnace, add argon gas for protection, keep the temperature at 960°C for 1.5 hours, and quench with water.

[0094] Step 4: Twin preparation: The alloy after the solution treatment is taken for twin preparation, and the alloy is subjected to multiple low-temperature dynamic plastic deformations using a Hopkinson pressure bar. The deformation temperature is in a liquid nitrogen environment (-196°C), and the final deformation amount ε = 2.1. During each deformation, the sample is immersed in liquid nitrogen temperature for 3 min.

[0095] Step 5. Introduction of precipitate phase: The alloy after twin preparation is taken for introduction of precipitate phase. The alloy is aged in a vacuum tube furnace to introduce the precipitate phase. Argon gas is used for protection throughout the aging process. After the temperature in the furnace is controlled to rise to 470°C, the sample is placed in a vacuum tube furnace for insulation treatment for 15 minutes. The sample is then taken out and cooled to room temperature to obtain a high-performance copper alloy with high-density twins and precipitate phases.

[0096] The performance test of the finished copper alloy obtained in this embodiment shows that its tensile strength is 796.4 MPa, the electrical conductivity is 45.1% IACS, and the elongation is 10.9%. (See Table 1 below).

[0097] Example 7

[0098] In this embodiment, a copper alloy with high-density twins and low mismatch precipitation phase is prepared. The copper alloy is composed of the following alloys in percentage by mass: 1.5% nickel, 0.7% cobalt, 0.65% silicon, and the balance copper.

[0099] The specific preparation method of the high performance copper alloy in this embodiment is:

[0100] Step 1: Alloy smelting:

[0101] According to the above alloy ratio, pure nickel, pure cobalt, pure silicon, pure chromium and the prepared standard electrolytic copper with a purity of not less than 99% are weighed respectively, put into a high-frequency vacuum melting furnace for melting, and evacuate the furnace until the pressure inside is 6×10 -2Pa, and then argon gas is injected to make the pressure in the furnace 0.03 MPa. Next, the temperature in the furnace is controlled at 1000°C, and casting is carried out at 900°C, and air-cooled to room temperature to form an alloy ingot for standby use;

[0102] Step 2, hot extrusion: heat the alloy ingot obtained in step 1 to 1050° C., keep it warm for 2 hours, and hot extrude it into a rod blank for standby use;

[0103] Step 3: Solution treatment: Place the rod blank obtained in step 2 into a box-type resistance furnace, add argon gas for protection, keep the temperature at 960°C for 1.5 hours, and quench with water.

[0104] Step 4: Twin preparation: The alloy after the solution treatment is taken for twin preparation, and the alloy is subjected to multiple low-temperature dynamic plastic deformations using a Hopkinson bar, the deformation temperature is in a liquid nitrogen environment (-196°C), and the final deformation amount ε = 2.2. During each deformation, the sample is immersed in liquid nitrogen temperature for 3 min.

[0105] Step 5. Introduction of precipitate phase: The alloy after twin preparation is taken for introduction of precipitate phase. The alloy is aged in a vacuum tube furnace to introduce the precipitate phase. Argon gas is used for protection throughout the aging process. After the temperature in the furnace is controlled to rise to 480°C, the sample is placed in a vacuum tube furnace for insulation treatment for 15 minutes. The sample is then taken out and cooled to room temperature to obtain a high-performance copper alloy with high-density twins and precipitate phases.

[0106] The performance test of the finished copper alloy obtained in this embodiment shows that its tensile strength is 787.6 MPa, the electrical conductivity is 44.3% IACS, and the elongation is 11.2%. (See Table 1 below).

[0107] Table 1 is a performance test comparison chart of various embodiments

[0108]

[0109] It can be seen from the above table that the high-performance copper alloy prepared by the present invention has significant advantages in tensile strength, electrical conductivity, elongation, etc., and has excellent comprehensive performance.

[0110] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A copper alloy having high-density twins and low mismatch precipitation phases, characterized in that: The invention comprises the following components in mass percentage: 1.0-1.5% Ni, 0.7-1.2% Co, 0.45-0.65% Si, and the balance is copper and inevitable impurity elements; the copper alloy contains 25-35% volume of high-density nano-scale twins, and the copper alloy is also uniformly distributed with nano-scale precipitated phases with a particle size of 2-5 nm, and the interface between the precipitated phase and the copper matrix has a mismatch of 0.5-0.75%; The method for preparing the copper alloy comprises the following steps: Step 1: Alloy smelting According to the above mass percentages, nickel, cobalt, silicon and copper are weighed respectively and placed in a high-frequency vacuum melting furnace, and are subjected to high-temperature vacuum melting under inert gas protection conditions. Thereafter, they are cast at 900-1100° C., and air-cooled to room temperature to obtain alloy ingots for standby use; Step 2: Hot extrusion The alloy ingot obtained in step 1 is heated to 900-1050°C for heat preservation for 2-3 hours, and then hot-extruded into a rod blank for standby use; Step 3: Solution treatment Under inert gas protection conditions, the rod blank obtained in step 2 is subjected to a heat preservation solid solution treatment in an environment of 900-960°C for 1.5-2h, and then water quenched; Step 4: Twinning Preparation The bar blank after water quenching in step 3 is subjected to multiple low-temperature dynamic plastic deformations at -196 ~ -150℃ by dynamic plastic deformation equipment, so that its final deformation ε > 1.9; where ε = ln (L0 / L f ), L0 is the initial height of the billet, L f is the final height of the billet after deformation; Step 5: Introduce the precipitated phase Under inert gas protection conditions, the sample prepared by twinning in step 4 is placed in a heating furnace at a temperature of 400-550°C for heat preservation and aging treatment for 10-15 min. After cooling to room temperature, a finished copper alloy with high-density twins and low mismatch precipitation phase is obtained.

2. The copper alloy having high-density twins and low mismatch precipitation phase according to claim 1, characterized in that: The mass ratio of (Ni+Co) / Si in the copper alloy is 4-4.

5.

3. The copper alloy with high-density twins and low mismatch precipitation phase according to claim 1, characterized in that: In step 1, before the high-temperature vacuum melting, the high-frequency vacuum melting furnace needs to be evacuated to a pressure of 8×10 -2 ~6×10 -2 Pa, and then, inert gas is filled in to make the pressure in the furnace 0.03~0.05 MPa.

4. The copper alloy with high-density twins and low mismatch precipitation phase according to claim 1 or 3, characterized in that: The inert gas is argon.

5. The copper alloy with high-density twins and low mismatch precipitation phase according to claim 1, characterized in that: In step 1, the temperature during high-temperature vacuum melting is 1000-1200°C.

6. The copper alloy with high-density twins and low mismatch precipitation phase according to claim 1, characterized in that: In step three, the heat preservation and solution treatment is carried out in a box-type resistance furnace.

7. The copper alloy with high-density twins and low mismatch precipitation phase according to claim 1, characterized in that: In step 4, during the low-temperature dynamic plastic deformation process, the rod blank needs to be cooled with liquid nitrogen for 3 to 5 minutes before each deformation.

8. The copper alloy with high-density twins and low mismatch precipitation phase according to claim 1, characterized in that: In step 4, the dynamic plastic deformation device is a Hopkinson pressure bar, and the strain rate of the dynamic plastic deformation device is greater than 10 -3 s -1 .

9. The copper alloy with high-density twins and low mismatch precipitation phase according to claim 1, characterized in that: In step 5, the heating furnace is a vacuum tube furnace, and the cooling process is performed in an air environment.