Conductive rubber compositions and articles comprising the thereof

By adding conductive carbon compounds to a rubber composition to form a continuous filler network, the balance between mechanical properties and conductivity in existing conductive rubber compositions is solved, resulting in a conductive rubber composition with low resistivity and good mechanical properties, suitable for a variety of applications.

CN116262841BActive Publication Date: 2026-11-17THE GOODYEAR TIRE & RUBBER CO
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211612200.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-12-15
Filing Date
2022-12-15
Publication Date
2026-11-17
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing conductive rubber compositions struggle to achieve good conductivity while maintaining acceptable mechanical reinforcement properties, being processable with existing equipment, and having conductivity that does not degrade over time.

Method used

By adding conductive carbon compounds such as carbon black, short carbon fibers, graphite powder, or graphene powder to a rubber composition to form a continuous filler network, a conductive rubber composition with good mechanical properties and resistivity can be prepared, which is suitable for processing with existing equipment.

Benefits of technology

A conductive rubber composition with low resistivity when molded into wires of specific sizes has been developed. It possesses good mechanical properties and does not degrade over time, making it suitable for a variety of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 142849DEST_PATH_IMAGE004
    Figure 142849DEST_PATH_IMAGE004
  • Figure 254025DEST_PATH_IMAGE001
    Figure 254025DEST_PATH_IMAGE001
  • Figure 809957DEST_PATH_IMAGE003
    Figure 809957DEST_PATH_IMAGE003
Patent Text Reader

Abstract

This invention discloses conductive rubber compositions and articles comprising the same. Conductive rubber compositions comprising a rubber component and one or more conductive carbon compounds are described herein. In another aspect, the conductive rubber composition can be prepared by first adding one or more conductive carbon components to a polymer phase, thereby creating a filler network in the continuous polymer phase of the finished product. In a further aspect, the conductive carbon component can be or includes one or more of the following: carbon black, short carbon fibers, graphite powder, or graphene powder. After mixing, the conductive rubber composition can optionally be vulcanized. The conductive rubber composition exhibits good mechanical properties and resistivity and can be processed using existing equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rubber, and more particularly to conductive rubber compositions and articles comprising the same. Background Technology

[0002] Many applications in computing, military, medical devices, telecommunications, and transportation require conductive rubber compounds. Although several methods have been proposed to obtain rubber compositions that meet the diverse needs of these industries, maintaining acceptable mechanical reinforcing properties has proven difficult.

[0003] Rubber is an electrical insulating material. To make rubber conductive, continuous pathways of conductive particles must be created within it. However, conductive fillers significantly affect the electrical and mechanical properties of rubber.

[0004] Furthermore, conductive carbon compounds are difficult to mix with high molecular weight rubbers and other polymers. Inhomogeneous mixing can lead to uneven distribution of the conductive carbon in articles made from the composition, affecting the conductivity of the rubber composition and its mechanical strength. Long carbon fibers can provide the required mechanical strength but lack elasticity and are prone to breakage.

[0005] Despite progress in the development of conductive rubbers, there remains a lack of conductive rubber compositions that possess acceptable mechanical properties, can be processed with existing equipment, and retain their conductivity without degradation over time. This disclosure addresses these and other needs. Summary of the Invention

[0006] This document describes a conductive rubber composition comprising a rubber component and one or more conductive carbon compounds, wherein the conductive rubber composition has an uncured or cured resistance of less than about 10 megohms (MΩ) at 23°C when molded into wires approximately 10 inches (254 mm) long and 2 mm in diameter. Alternatively, the conductive rubber composition can be prepared by first adding one or more conductive carbon components to a polymer phase, thereby creating a filler network in the continuous polymer phase of the finished product. In a further aspect, the conductive carbon component can be or include one or more of the following: carbon black, short carbon fibers, graphite powder, or graphene powder. After mixing, the conductive rubber composition can optionally be vulcanized. The conductive rubber composition exhibits good mechanical properties and resistivity and can be processed using existing equipment. Articles comprising the conductive rubber composition are also disclosed.

[0007] The present invention discloses the following embodiments: 1. A conductive rubber composition comprising a rubber component and one or more conductive carbon components, wherein the conductive rubber composition has an uncured or cured resistance of less than about 10 MΩ at 23°C when molded into a wire of about 10 inches (254 mm) in length and 2 mm in diameter.

[0008] 2. The conductive rubber composition according to Scheme 1, wherein the rubber component comprises natural rubber (NR), polyisoprene rubber (IR), styrene-butadiene rubber (SBR), polybutadiene rubber (BR), butyl or halogenated butyl rubber, ethylene propylene rubber (EM), ethylene propylene diene monomer (EPDM), chloroprene rubber (CR), nitrile rubber (NBR), hydrogenated acrylonitrile butadiene rubber (HNBR), silicone rubber (MQ), thermoplastic rubber, or any combination thereof.

[0009] 3. The conductive rubber composition according to Scheme 2, wherein the butyl or halogenated butyl rubber comprises isobutylene-isoprene rubber (IIR), brominated isobutylene-isoprene rubber (BIIR), chlorinated isobutylene-isoprene rubber (CIIR), brominated isobutylene-co-p-methylstyrene rubber (BIMS), or any combination thereof.

[0010] 4. The conductive rubber composition according to Scheme 1, wherein the conductive rubber composition comprises a blend of two or more rubber components.

[0011] 5. The conductive rubber composition according to Scheme 1, wherein the rubber component comprises approximately 5 × 10⁻⁶ 4 Da up to approximately 3 × 10 7 The molecular weight of Da (M) w ).

[0012] 6. The conductive rubber composition according to Scheme 1, wherein the rubber component comprises a Mooney viscosity UML of about 0.01 to about 150 or a Mooney viscosity UMS of about 2 to about 150.

[0013] 7. The conductive rubber composition according to Scheme 1, wherein the rubber component comprises a glass transition temperature of about -110°C to about 30°C.

[0014] 8. The conductive rubber composition according to claim 1, wherein the rubber component comprises a molecular weight distribution of about 1 to about 10 (M w / M n ).

[0015] 9. The conductive rubber composition according to Scheme 1, wherein the one or more conductive carbon components comprise carbon black, short carbon fibers, graphite powder, graphene powder, or any combination thereof.

[0016] 10. The conductive rubber composition according to Scheme 1, wherein the one or more conductive carbon components are present in an amount of about 20 phr to about 150 phr.

[0017] 11. The conductive rubber composition according to Scheme 1, wherein the one or more conductive carbon components comprise an average particle size of about 5 nm to about 100 nm and about 20 nm. 2 / g to approximately 1700 m 2 / g of BET surface area carbon black.

[0018] 12. The conductive rubber composition according to Scheme 1, wherein the one or more conductive carbon components comprise carbon fibers, wherein the carbon fibers comprise chopped carbon fiber yarns, multi-walled carbon nanotubes (MWCNTs), single-walled carbon nanotubes (SWCNTs), or any combination thereof.

[0019] 13. The conductive rubber composition according to Scheme 12, wherein the short carbon fibers have a diameter of about 1 nm to about 1000 nm and a diameter of about 1 μm to about 1 × 10⁻⁶. 4 The length is μm.

[0020] 14. The conductive rubber composition according to Scheme 1, wherein the one or more carbon components comprise a blend of carbon black and short carbon fibers.

[0021] 15. The conductive rubber composition according to claim 14, wherein, in the blend, the short carbon fibers are from about 5 phr to about 80 phr, and the carbon black is from about 15 phr to about 70 phr.

[0022] 16. The conductive rubber composition according to Scheme 1, further comprising at least one additional component selected from antioxidants, anti-ozone agents, oils, zinc oxide, fatty acids, sulfur, accelerators, anti-scorching agents, or any combination thereof.

[0023] 17. The conductive rubber composition according to Scheme 1, wherein the conductive rubber composition has a tensile strength of about 2 MPa to about 30 MPa.

[0024] 18. The conductive rubber composition according to claim 1, wherein the conductive rubber composition has an elongation at break of about 200% to about 800%.

[0025] 19. An article comprising the conductive rubber composition according to claim 1.

[0026] 20. The article of claim 19, wherein the article comprises a tire, a tire chimney, a wire, a sensor, a hose, an electromagnetic interference shielding gasket, a weather-resistant sealing material, an adhesive article, or any combination thereof.

[0027] Other systems, methods, features, and advantages of this disclosure will be apparent to those skilled in the art upon examination of the following drawings and detailed description. All such additional systems, methods, features, and advantages are intended to be included in this specification, within the scope of this disclosure, and protected by the appended claims. Furthermore, all optional and preferred features and modifications of the described embodiments are applicable to all aspects of this disclosure taught herein. Moreover, the various features of the dependent claims, as well as all optional and preferred features and modifications of the described embodiments, are combinable and interchangeable with each other. Detailed Implementation

[0028] In one aspect, this document discloses a conductive rubber composition comprising a rubber component and one or more conductive carbon compounds. In another aspect, this conductive rubber composition can be prepared by first adding one or more conductive carbon components to a polymer phase, thereby creating a filler network in the continuous polymer phase of the finished product. In a further aspect, the conductive carbon component can be or includes one or more of the following: carbon black, short carbon fibers, graphite powder, or graphene powder. After mixing, the conductive rubber composition can optionally be vulcanized. This conductive rubber composition has acceptable mechanical properties and conductivity and can be processed using existing equipment.

[0029] definition As used herein, “comprising” is to be interpreted as specifying the presence of the mentioned feature, integer, step, or component, but does not preclude the presence or addition of one or more features, integers, steps, or components, or groups thereof. Furthermore, the terms “by,” “comprising,” “comprises,” “comprised of,” “including,” “includes,” “included,” “involving,” “involves,” “involved,” and “for example” are each used in their open, non-restrictive sense and may be used interchangeably. Additionally, the term “comprising” is intended to include instances and aspects covered by the terms “substantially constitutes” and “consistent with.” Similarly, the term “substantially constitutes” is intended to include instances covered by the term “consistent with.”

[0030] As used in the specification and appended claims, the singular forms “a,” “an,” and “the” include plural objects unless the context clearly specifies otherwise. Thus, for example, references to “a conductive carbon compound,” “a rubber component,” or “an oil” include, but are not limited to, mixtures or combinations of two or more such conductive carbon compounds, rubber components, or oils, etc.

[0031] It should be noted that ratios, concentrations, amounts, and other numerical data may be expressed in range format herein. It should be further understood that each endpoint of a range is significant in relation to and independent of another endpoint. It should also be understood that there are many values ​​disclosed herein, and each value is also disclosed herein as having an "approximately" value in addition to itself. For example, if the value "10" is disclosed, then "approximately 10" is also disclosed. A range herein may be expressed as from "approximately" one specific value, and / or to "approximately" another specific value. Similarly, when a value is expressed as an approximation using the antecedent "approximately," it should be understood that the specific value forms a further aspect. For example, if the value "approximately 10" is disclosed, then "10" is also disclosed.

[0032] When indicating a range, a further aspect includes from one specific value and / or to another specific value. For example, when the range includes one or two boundaries, this disclosure also includes ranges excluding any one or both of those included boundaries, such as the phrase "x to y" which includes a range from "x" to "y" as well as ranges greater than "x" and less than "y". The range can also be expressed as an upper limit, such as "approximately x, y, z or less", and should be interpreted as including the specific ranges of "approximately x", "approximately y", and "approximately z", as well as the ranges of "less than x", "less than y", and "less than z". Similarly, the phrase "approximately x, y, z or greater" should be interpreted as including the specific ranges of "approximately x", "approximately y", and "approximately z", as well as the ranges of "greater than x", "greater than y", and "greater than z". Furthermore, the phrase "approximately 'x' to 'y'", where 'x' and 'y' are numerical values, includes "approximately 'x' to approximately 'y'".

[0033] It should be understood that this range format is used for convenience and brevity, and therefore should be interpreted flexibly to include not only the values ​​explicitly listed as range boundaries, but also all individual values ​​or subranges covered within that range, as if each value and subrange were explicitly stated. For example, the range “approximately 0.1% to 5%” should be interpreted to include not only the explicitly listed values ​​of approximately 0.1% to approximately 5%, but also individual values ​​(e.g., approximately 1%, approximately 2%, approximately 3%, and approximately 4%) and subranges (e.g., approximately 0.5% to approximately 1.1%; approximately 5% to approximately 2.4%; approximately 0.5% to approximately 3.2%, and approximately 0.5% to approximately 4.4%, and other possible subranges) within the specified range.

[0034] As used herein, the terms “approximately,” “roughly,” “equal to or approximately,” and “substantially” mean that the relevant quantity or value may be an exact value or a value that provides an equivalent result or effect as described in the claims or taught herein. That is, it is to be understood that quantities, dimensions, formulations, parameters, and other quantities and characteristics are not and need not be exact, but may be approximate and / or larger or smaller as required, reflecting tolerances, conversion factors, rounding, measurement errors, and other factors known to those skilled in the art in order to obtain an equivalent result or effect. In some cases, it is not reasonable to determine a value that provides an equivalent result or effect. In such cases, it is generally understood that, unless otherwise indicated or inferred, “approximately” and “equal to or approximately” as used herein refer to nominal values ​​indicating a variation of ±10%. Generally, whether explicitly stated or not, quantities, dimensions, formulations, parameters, or other quantities or characteristics are “approximately,” “roughly,” or “equal to or approximately.” It is to be understood that, unless specifically stated otherwise, when “approximately,” “roughly,” or “equal to or approximately” is used before a quantitative value, the parameter also includes the specific quantitative value itself.

[0035] As used herein, the term "effective amount" refers to an amount sufficient to achieve the desired change in the physical properties of a composition or material. For example, the "effective amount" of a conductive carbon compound refers to an amount sufficient to achieve the desired improvement in properties regulated by the formulation components (e.g., achieving a desired resistivity level). The specific level in the composition required as an effective amount, expressed as a percentage by weight, will depend on a variety of factors, including the amount and type of rubber component, the molecular weight of the rubber component, the form and size of the conductive carbon compound, and the end use of any article made using the conductive rubber composition.

[0036] As used herein, the terms “optional” or “optionally” mean that the event or condition described below may or may not occur, and the description includes both cases in which the event or condition occurs and cases in which the event or condition does not occur.

[0037] "Resistance" refers to how strongly a material, such as conductive rubber, resists the flow of electric current. Materials with high resistance are better insulators, while materials with low resistance are better conductors. Resistance can be measured using standard instruments, such as the FLUKE 117 true RMS multimeter.

[0038] "Elongation at break" refers to the percentage of the original length of a rubber or elastomer material to the length it extends to at break when a stretching or tensile force is applied to the material.

[0039] "Fiber" is a natural or man-made unit of matter that is the basic element that forms a filament, characterized in that its length is at least 10 times its diameter or width.

[0040] "Modulus" refers to the tension at a specific elongation value when a rubber or elastomer material is subjected to stretching or tensile motion (e.g., 10% modulus, 50% modulus, etc.).

[0041] "Mounney viscosity" refers to the shear torque required to resist the rotation of a cylindrical metal disk or rotor embedded in a cylindrical cavity within rubber, and is reported in arbitrary Mooney units. An exemplary procedure for determining Mooney viscosity can be found in the standard test method ASTM D 1646.

[0042] “Phr” refers to the number of parts by weight of the corresponding material per 100 parts by weight of rubber or elastomer.

[0043] Storage modulus (G') is a measure of the deformation energy stored elastically in a viscoelastic material. In some respects, materials with a higher degree of cross-linking will have a larger storage modulus.

[0044] "T25" refers to the curing time required for the rubber composition to reach 25% of its ultimate elastic torque, expressed in minutes with reference to a given temperature. Meanwhile, "T90" is the time required for the rubber composition to reach 90% of its ultimate elastic torque value. T25 and T90 can be measured using a moving die rheometer and / or a rubber processing analyzer.

[0045] "Zwick rebound" refers to a test of a material's elasticity. In this test, a force is applied to the material. A perfectly elastic material stores the energy from the force and releases it when the force is removed. A perfectly plastic material absorbs the energy provided. Rubber materials typically have a Zwick rebound value that reflects their degree of plasticity and elasticity, and the Zwick rebound value generally varies with temperature.

[0046] As used in this article, “oil absorption value” refers to the number of cubic centimeters or milliliters of dibutyl phthalate (DBP) or paraffin oil absorbed by 100 grams of carbon black under a set of standard conditions.

[0047] Unless otherwise stated, the pressures mentioned in this article are based on atmospheric pressure (i.e., one atmosphere).

[0048] rubber components In one aspect, the conductive rubber composition disclosed herein includes a rubber component. In a further aspect, the rubber component may be natural rubber (NR), polyisoprene rubber (IR), styrene-butadiene rubber (SBR), polybutadiene rubber (BR), butyl or halogenated butyl rubber, ethylene propylene rubber (EM), ethylene propylene diene monomer (EPDM), chloroprene rubber (CR), nitrile rubber (NBR), hydrogenated acrylonitrile butadiene rubber (HNBR), silicone rubber (MQ), thermoplastic rubber, or any combination thereof. In a further aspect, the butyl or halogenated butyl rubber may be isobutylene-isoprene rubber (IIR), brominated isobutylene-isoprene rubber (BIIR), chlorinated isobutylene-isoprene rubber (CIIR), brominated isobutylene-co-p-methylstyrene rubber (BIMS), or any combination thereof. In another aspect, the thermoplastic rubber may be poly(styrene-butadiene-styrene) rubber (SBS), thermoplastic elastomer rubber (TPE), melt-processable rubber (MPR), or any combination thereof. On the one hand, thermoplastic elastomer rubber can be thermoplastic polyurethane rubber.

[0049] On the one hand, conductive rubber compositions comprise blends of two or more rubber components. On the other hand, and without being bound by theory, conductive systems based on polymer blends can achieve high conductivity with lower filler content, thereby alleviating the difficulties of blending carbon compounds in polymers and reducing material costs.

[0050] molecular weight On one hand, the rubber component can have approximately 5 × 10⁻⁶. 4 Da up to approximately 3 × 10 7 Da, or approximately 3 × 10 5 Da up to approximately 5 × 10 6 Da, or approximately 5 × 10 4 Da, 6 × 10 4 Da, 7 × 10 4 Da, 8 × 10 4 Da, 9 × 10 4 Da, 1 × 10 5 Da, 2 × 10 5 Da, 3 × 10 5 Da, 4 × 10 5 Da, 5 × 10 5 Da, 6 × 10 5 Da, 7 × 10 5 Da, 8 × 10 5 Da, 9 × 10 5 Da, 1 × 106 Da, 2 × 10 6 Da, 3 × 10 6 Da, 4 × 10 6 Da, 5 × 10 6 Da, 6 × 10 6 Da, 7 × 10 6 Da, 8 × 10 6 Da, 9 × 10 6 Da, 1 × 10 7 Da, 2 × 10 7 Da, or approximately 3 × 10 7 Da, or any combination of the foregoing values, or a molecular weight (M) covering a range of the foregoing values. w ).

[0051] Molecular weight distribution On the other hand, the rubber component may have a molecular weight distribution (M0) of about 1 to about 10, or about 2.1 to about 10, or about 3.9 to about 8.2, or about 1, 1.25, 1.5, 1.75, 2, 2.1, 2.25, 2.5, 2.75, 3, 3.25, 3.5, 3.75, 4, 4.25, 4.5, 4.75, 5, 5.25, 5.5, 5.75, 6, 6.25, 6.5, 6.75, 7, 7.25, 7.5, 7.75, 8, 8.25, 8.5, 8.75, 9, 9.25, 9.5, 9.75, or about 10, or any combination of the foregoing values, or covering a range of any of the foregoing values. w / M n ).

[0052] Mooney viscosity On one hand, the rubber component has a Mooney viscosity UML of about 0.01 to about 150, or about 0.01, 0.05, 0.1, 0.5, 1, 2, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 145, or about 150, or any combination of the foregoing values, or a range covering any of the foregoing values. On the other hand, the rubber component has a Mooney viscosity UMS of about 2 to about 150, or about 2, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 145, or about 150, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0053] Glass transition temperature (T) g ) On one hand, the rubber component has a glass transition temperature of about -110°C to about 30°C, or about -75°C to about -25°C, or about -110, -105, -100, -95, -90, -85, -80, -75, -70, -65, -60, -55, -50, -45, -40, -35, -30, -25, -20, -15, -10, -5, 0, 5, 10, 15, 20, 25, or about 30°C, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0054] Exemplary rubber components On one hand, in the disclosed conductive rubber composition, the rubber component comprises components with a molecular weight of approximately 3 × 10⁻⁶. 4 Da up to approximately 3 × 10 7 Natural rubber with a glass transition temperature of approximately -75°C to approximately -65°C.

[0055] On one hand, in the disclosed conductive rubber composition, the rubber component comprises components with a molecular weight of approximately 2 × 10⁻⁶. 5 Da up to approximately 8 × 10 5 Synthetic cis-1,4-polyisoprene rubber with a Da, Mooney viscosity UML of approximately 75 and a glass transition temperature of approximately -70°C to approximately -60°C.

[0056] On one hand, in the disclosed conductive rubber composition, the rubber component comprises components with a molecular weight of approximately 1 × 10⁻⁶. 5 Da up to approximately 4 × 10 5Styrene-butadiene rubber produced by emulsion polymerization with a Da, Mooney viscosity of approximately 50 UML, and a glass transition temperature of approximately -60°C to approximately -50°C.

[0057] On one hand, in the disclosed conductive rubber composition, the rubber component comprises components with a molecular weight of approximately 7 × 10⁻⁶. 4 Da up to approximately 8 × 10 4 Styrene-butadiene rubber is a solution polymerized styrene-butadiene rubber with a Da, Mooney viscosity UML of about 2.6 and a glass transition temperature of about -30°C to about -20°C.

[0058] Exemplary suitable rubber components include, but are not limited to, the following: TSR20 natural rubber, RSS natural rubber, NATSYN 2200, PLF1502, Exp SBR, and combinations thereof. In one aspect, TSR20 (Technical Grade Rubber) natural rubber is a block rubber available from multiple manufacturers, primarily composed of cis-1,4-polyisoprene and having a TSR20 temperature range of -70°C. g It has a molecular weight distribution of 4.59 to 8.11, a Mooney viscosity (UML) of 88 to 99.2, and a maximum impurity (dirt) of 20%. On the other hand, RSS (#2 Ribbed Smoked Sheet Rubber) is a form of raw natural rubber available from multiple manufacturers and has a T70°C temperature range. g Natural rubber exhibits a molecular weight distribution of 1.35 to 2.36 and a Mooney viscosity (UMS) of 80 to 142. In any of these respects, the molecular weight range of natural rubber can be approximately 1 × 10⁻⁶. 7 Da up to approximately 3 × 10 7 On another note, NATSYN 2200 (Goodyear Chemical, Akron OH) is a synthetic high-cis polyisoprene containing a non-staining antioxidant and a T0 of -64°C. g 2.04 × 10 5 Da's M n 7.31 × 10 3 Da's M w It has a molecular weight distribution of 3.575 and a Mooney viscosity (UML) of 75. On one hand, PLF1502 (PLIOFLEX 1502, Goodyear Chemical, Akron OH) is an emulsion-polymerized styrene-butadiene copolymer (23.5% styrene, 12% vinyl, 55% trans, 10% cis) with a T55 temperature range. g1.01 × 10 5 Da's M n 4.03 × 10 5 Da's M w With a molecular weight distribution of 3.99 and a Mooney viscosity (UML) of 50, it contains non-polluting antioxidants. On one hand, Exp SBR is an experimental Li-solution-based styrene-butadiene rubber with a T0 of -26°C. g 7.39 × 10 4 Da's M n 7.39 × 10 4 Da's M w , 1.00 molecular weight distribution and 2.63 Mooney viscosity (UML).

[0059] carbon compounds In one respect, the conductive rubber compositions disclosed herein comprise a conductive carbon component. Exemplary conductive carbon components are described below.

[0060] In one respect, one or more carbon components may be present in amounts ranging from about 20 phr to about 150 phr, or from about 30 phr to about 100 phr, or from about 40 phr to about 80 phr, or in amounts ranging from about 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, or about 150 phr, or any combination of the foregoing values, or in amounts covering a range of the foregoing values.

[0061] carbon black On one hand, the conductive carbon component may be or include carbon black. On the other hand, the carbon black may have a particle size of about 5 nm to about 100 nm, or about 5 nm to about 50 nm, or about 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or about 100 nm, or any combination of the foregoing values, or an average particle size covering a range of any of the foregoing values.

[0062] On the one hand, carbon black can have approximately 20 μm 2 / g to approximately 1700 m 2 / g, or approximately 50 mg 2 / g to approximately 1500m 2 / g, or approximately 20, 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600, or approximately 1700 m 2 / g, or any combination of the foregoing values, or the BET surface area covering a range of the foregoing values.

[0063] On the other hand, carbon black can have a density of approximately 20 to approximately 1200 μm. 2 / g, or approximately 100 m 3 / g to approximately 300 m 3 / g, or approximately 150 mg 3 / g to approximately 200 m 3 / g, or approximately 20, 25, 50, 75, 100, 125, 150, 175, 200, 225, 250, 275, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1050, 1100, 1150, or approximately 1200 m 3 / g, or any combination of the aforementioned values, or the external surface area based on the statistical thickness method (STSA) covering a range of the aforementioned values.

[0064] On the other hand, carbon black may have an oil absorption value of about 500 mL / 100 g to about 20 mL / 100 g, or about 500 mL / 100 g to about 80 mL / 100 g, or about 500, 450, 400, 350, 300, 250, 200, 150, 100, or about 80 mL / 100 g, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0065] Suitable carbon blacks, including but not limited to, are: N299 ASTM grade carbon black, PRINTEX XE2B (Orion Engineered Carbons, Luxembourg), PROPEL X22 (Cabot Corporation, Boston MA), or any combination thereof. In one aspect, PRINTEX XE2B has an oil absorption value of 410 mL / 100g as measured by standard test method ASTM D 2414 and an oil absorption value of 1100 mL / 100g as measured by ASTM D 6556. 2 PROPEL X22 has a BET surface area of ​​230 mg / g and an average primary particle size of 30 nm based on ASTM D 3849. On the other hand, PROPEL X22 has an iodine value of 230 mg / g according to standard test method ASTM D 1510 and an iodine value of 173 mg / g according to standard test method ASTM D6556. 2 / g based on statistical thickness method external surface area (STSA), oil absorption value of 100 mL / 100 g compressed sample (COAN) according to standard test method ASTM D3493, and coloration of 150% ITRB according to standard test method ASTM D 3265. Other available carbon blacks include BLACK PEARLS 2000 carbon black and Vulcan XC-72 (BOTH FROM Cabot Corporation, Boston MA), CONDUCTEX 975 and CONDUCTEXSC (Columbian Chemicals, Hamilton ON Canada), and PRINTEX XE2, PRINTEX L and PRINTEX L6 (Orion Engineered Carbons, Luxembourg).

[0066] short carbon fiber In one aspect, the conductive carbon component may be or include short carbon fibers. In another aspect, the short carbon fibers may be carbon fibers, chopped carbon fiber yarns, multi-walled carbon nanotubes (MWCNTs), single-walled carbon nanotubes (SWCNTs), or any combination thereof. In another aspect, the short carbon fibers have a diameter of about 1 nm to about 1000 nm, or about 150 nm to about 600 nm, or about 1, 10, 25, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950 nm, or about 1000 nm, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0067] On the other hand, short carbon fibers can have a diameter from approximately 1 μm to approximately 1 × 10⁻⁶. 4 μm, or approximately 1, 100, 500, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, or approximately 10,000 μm, or any combination of the foregoing values, or the length of a range covering any of the foregoing values.

[0068] In another aspect, the short carbon fibers may have a ratio of approximately 10:1 to approximately 10,000:1, or approximately 10:1, 50:1, 100:1, 500:1, 1000:1, 2000:1, 3000:1, 4000:1, 5000:1, 6000:1, 7000:1, 8000:1, 9000:1, or approximately 10,000:1, or any combination of the foregoing values, or an average lateral length to thickness ratio covering a range of the foregoing values.

[0069] Exemplary short carbon fibers used in this article have a diameter of approximately 150 to approximately 600 nm (depending on grade) and a length of approximately 120–190 m. 2 / g of BET surface area and length greater than 1 μm.

[0070] blends In some respects, the carbon component may include blends. In one respect, one or more carbon components consist of blends of carbon black and graphite powder, or blends of carbon black and graphene powder.

[0071] On the other hand, one or more carbon components include blends of carbon black and short carbon fibers. On one hand, and not wishing to be bound by theory, blends containing carbon black and short carbon fibers can provide additional advantages in terms of the conductivity of the mixture. On one hand, carbon black can improve inter-fiber contact by forming particle bridges, while carbon fibers can help electrons transport over long distances, thereby creating a continuous path for electrical conduction in the disclosed composition. On some aspects, blends containing carbon black and short carbon fibers can result in different conductive network structures in polymer blends compared to rubber compositions based on a single polymer.

[0072] Furthermore, in this respect, the short carbon fibers can be from about 5 phr to about 80 phr, or from about 20 phr to about 40 phr, or can be about 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, or about 80 phr, or any combination of the foregoing values, or a range covering any of the foregoing values, and the carbon black can be from about 15 phr to about 70 phr, or from about 10 phr to about 60 phr, or about 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, or about 70 phr, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0073] On one hand, the conductive carbon component may include ASTM N299 grade carbon black with a diameter of approximately 1 nm to approximately 1000 nm and a particle size of approximately 1 μm to approximately 1 × 10⁻⁶. 4 Short carbon fibers with a length of μm.

[0074] On the other hand, the conductive carbon component may include carbon black having an oil absorption value of approximately 100 mL / 100 g and a diameter of approximately 1 nm to approximately 1000 nm and a particle size of approximately 1 μm to approximately 1 × 10⁻⁶ g. 4 Short carbon fibers with a length of μm.

[0075] On the other hand, the conductive carbon component may include carbon black having an average particle size of about 30 nm and a diameter of about 1 nm to about 1000 nm and a particle size of about 1 μm to about 1 × 10⁻⁶. 4 Short carbon fibers with a length of μm.

[0076] Additional components In one respect, in addition to the components already described, the conductive rubber compositions disclosed herein may additionally contain one or more additional components. In another respect, the additional components may be selected from antioxidants and / or anti-ozone agents, oils, zinc oxide, fatty acids, sulfur, accelerators, retarders, and combinations thereof.

[0077] Antioxidants and / or anti-ozone agents In one aspect, the conductive rubber composition disclosed herein comprises at least one antioxidant, at least one anti-ozone agent, or any combination thereof. In one aspect, the anti-ozone agent protects the rubber composition from ozone (O3). In another aspect, the anti-ozone agent can be a material that migrates to the surface of a rubber article to protect it from ozone, such as a wax. Suitable examples of anti-ozone agents include, but are not limited to, Antiozite 67P (Vanderbilt Chemicals, LLC, Norwalk CT USA). In one aspect, the antioxidant is a non-polluting antioxidant. In another aspect, the antioxidant can be an amine antioxidant, a diphenylamine antioxidant, a polymeric dihydroquinoline, or any combination thereof. In yet another aspect, the antioxidant or anti-ozone agent may be present in the composition in an amount from about 1 phr to about 2 phr, or in an amount of about 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or about 2 phr, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0078] Oil In one aspect, the conductive rubber composition contains an oil. In another aspect, the oil is a standard rubber processing oil, such as an aromatic rubber processing oil, a paraffinic rubber processing oil, a naphthenic rubber processing oil, or any combination thereof. In one aspect, the rubber processing oil can improve the dispersion of fillers and the flow properties of the rubber composition during processing. In one aspect, the oil may be present in an amount from about 4 phr to about 30 phr, or in an amount of about 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or about 30 phr, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0079] Zinc oxide In one aspect, the conductive rubber composition disclosed herein comprises zinc oxide. In another aspect, zinc oxide is an activator that can be used for rubber vulcanization. In one aspect, zinc oxide is present in the conductive rubber composition in an amount of about 1 phr to about 5 phr, or in an amount of about 1, 2, 3, 4, or about 5 phr, or any combination of the foregoing values, or a range covering any of the foregoing values. In one aspect, zinc oxide is present in an amount of about 3 phr.

[0080] fatty acid In one aspect, the conductive rubber composition disclosed herein comprises fatty acids. In another aspect, the fatty acids may be stearic acid, palmitic acid, oleic acid, or any combination thereof. In a further aspect, the fatty acids may be present in the conductive rubber composition in an amount from about 1 phr to about 5 phr, or in an amount of about 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.25, 2.5, 2.75, 3, 3.25, 3.5, 3.75, 4, 4.25, 4.5, 4.75, or about 5 phr, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0081] sulfur In one aspect, the conductive rubber composition disclosed herein contains sulfur. In another aspect, sulfur may be present in amounts from 0.5 to about 5 phr, or from about 0.5 to about 3 phr, or in amounts of about 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or about 5 phr, or any combination of the foregoing values, or a range covering any of the foregoing values. In one aspect, sulfur is present in an amount of about 1.8 phr. In one aspect, sulfur can be used to form crosslinks between rubber chains during a vulcanization process.

[0082] Accelerator In one aspect, the conductive rubber composition includes an accelerator. In another aspect, the accelerator may be a sulfenamide sulfur curing accelerator. In another aspect, the accelerator is present in an amount of about 0.5 to about 5 phr, or about 1 to about 2 phr, or in an amount of about 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or about 5 phr, or any combination of the foregoing values, or a range covering any of the foregoing values. In another aspect, the accelerator is present in an amount of about 1.2 phr.

[0083] Anti-scorching agent In one aspect, the conductive rubber composition contains an anti-scorching agent. In another aspect, the anti-scorching agent may be N-(cyclohexylthio)phthalimide. In yet another aspect, the anti-scorching agent may be present in an amount of about 0.05 to about 0.5 phr, or about 0.1 phr to about 0.3 phr, or in an amount of about 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, or about 0.5 phr, or any combination of the foregoing values, or an amount covering a range of the foregoing values.

[0084] On the one hand, anti-scorching agents can be used to prevent premature vulcanization during rubber processing. An exemplary anti-scorching agent could be Vantard PVI (Vanderbilt Chemicals, LLC, Norwalk CT USA).

[0085] Method for preparing conductive rubber compositions In one aspect, the disclosed conductive rubber composition can be prepared by mixing one or more additives into a rubber or a polymer base of a rubber composition. In a further aspect, the rubber or polymer base of a rubber composition is heated to soften it sufficiently to allow the additives to be mixed into the rubber composition. In yet another aspect, additives are discussed herein, and the additives include one or more of antioxidants or anti-ozone agents, oils, zinc oxide, fatty acids, sulfur, accelerators, scorch inhibitors, and one or more conductive carbon components.

[0086] In one respect, additives can be mixed into the rubber composition sequentially or simultaneously. In some respects, a masterbatch containing non-reactive additives such as conductive carbon components can be prepared to ensure that the conductive carbon components are fully mixed before vulcanization begins. In a further respect, vulcanizing additives (e.g., sulfur, zinc oxide) can be added to the masterbatch after its preparation.

[0087] In some respects, the rubber composition may be further shaped before or during the early stages of vulcanization by means including but not limited to extrusion, calendering, molding, casting, another rubber processing method or any combination thereof.

[0088] In some respects, processing aids, such as waxes, including but not limited to microcrystalline waxes and paraffin waxes, may be used, if used, in the range of, for example, about 1 phr to about 5 phr, or about 1 phr to about 3 phr, or about 1, 2, 3, 4, or about 5 phr, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0089] On the other hand, a resin (usually as a tackifier) ​​may be incorporated into the rubber composition, wherein the tackifier or resin is a compound such as synthetic hydrocarbons and natural resins, if used, ranging, for example, from about 1 phr to 5 phr or from about 1 phr to about 3 phr, or from about 1, 2, 3, 4, or about 5 phr, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0090] In some respects, the curing agent may be present as sulfur in conjunction with one or more sulfur curing accelerators. In other respects, for a sulfur and (one or more) accelerator curing agent, the amount of sulfur used may be, for example, from about 0.5 phr to about 5 phr, or from about 0.5 to about 3 phr, or in the range of about 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or about 5 phr, or any combination of the foregoing values, or a range covering any of the foregoing values; and (one or more) accelerators (typically of the sulfenamide type) are used in the range of about 0.5 phr to about 5 phr, or from about 1 phr to about 2 phr, or in the range of about 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or about 5 phr, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0091] In another aspect, the components of the composition, including the elastomer but excluding sulfur and accelerators / curing agents, are typically first mixed together in a series of at least two sequential mixing stages, although sometimes a single mixing stage may be used, to a temperature range, for example, from about 145°C to about 185°C, or about 145, 150, 155, 160, 165, 170, 175, 180, or about 185°C, or any combination of the foregoing values, or a range covering any of the foregoing values, and such a mixing stage is generally referred to as a non-productive mixing stage. In a further aspect, sulfur and accelerators, along with optionally one or more scorch inhibitors and optionally one or more anti-degradation agents, are mixed in a second stage, generally referred to as a productive mixing stage, to a temperature range, for example, from about 90°C to about 120°C, or about 90, 95, 100, 105, 110, 115, or about 120°C, or any combination of the foregoing values, or a range covering any of the foregoing values. Such mixing procedures are well known to those skilled in the art.

[0092] Properties of conductive rubber compositions Uncured energy storage modulus In one aspect, the disclosed conductive rubber composition may have an uncured storage modulus of about 185 kPa to about 1100 kPa, or about 185, 200, 300, 400, 500, 600, 700, 800, 900, 1000, or about 1100 kPa, or any combination of the foregoing values, or a range covering any of the foregoing values, at 15% strain, 100°C, and 0.83 Hz. In a further aspect, the uncured storage modulus can be measured using a rubber processing analyzer.

[0093] Energy storage modulus In one aspect, the disclosed conductive rubber composition may have a storage modulus at 1% strain, 100°C and 11 Hz that is from about 1.1 MPa to about 4 MPa, or about 1.1, 1.5, 2, 2.5, 3, 3.5 or about 4 MPa, or any combination of the foregoing values, or covering a range of the foregoing values.

[0094] In one aspect, the disclosed conductive rubber composition may have a storage modulus of about 0.8 MPa to about 3 MPa, or about 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, or about 3 MPa, or any combination of the foregoing values, or a range covering any of the foregoing values ​​at 10% strain, 100°C, and 11 Hz.

[0095] In one respect, the disclosed conductive rubber composition may have a storage modulus of about 0.35 MPa to about 1 MPa, or about 0.35, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or about 1 MPa, or any combination of the foregoing values, or a range covering any of the foregoing values ​​at 50% strain, 100°C and 11 Hz.

[0096] In any of these respects, the energy storage modulus can be measured using a rubber processing analyzer.

[0097] Modulus In one respect, the disclosed conductive rubber composition may have a modulus of about 0.4 MPa to about 2.5 MPa, or about 0.4, 0.5, 1, 1.5, 2, or about 2.5 MPa, or any combination of the foregoing values, or 10% of the range covering any of the foregoing values.

[0098] On the other hand, the disclosed conductive rubber composition may have a modulus of about 1.25 MPa to about 3.5 MPa, or about 1.25, 1.5, 2, 2.5, 3, or about 3.5 MPa, or any combination of the foregoing values, or 50% of the range covering any of the foregoing values.

[0099] In another aspect, the disclosed conductive rubber composition may have a modulus of about 2 MPa to about 5.2 MPa, or about 2, 2.5, 3, 3.5, 4, 4.5, 5, or about 5.2 MPa, or any combination of the foregoing values, or 100% of a range covering any of the foregoing values.

[0100] In one respect, the disclosed conductive rubber composition may have a modulus of about 3 MPa to about 12 MPa, or about 3, 4, 5, 6, 7, 8, 9, 10, 11, or about 12 MPa, or any combination of the foregoing values, or 200% of the range covering any of the foregoing values.

[0101] In one respect, the disclosed conductive rubber composition may have a modulus of about 4 MPa to about 13.5 MPa, or about 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, or about 13.5 MPa, or any combination of the foregoing values, or 300% of the range covering any of the foregoing values.

[0102] In any of these respects, the modulus can be measured using a tensile test based on ASTM D 412.

[0103] Tensile strength In one respect, the conductive rubber compositions disclosed herein may have tensile strengths greater than about 2 MPa, or from about 2 MPa to about 30 MPa, or about 2, 2.5, 3, 3.5, 4, 4.5, 5, 10, 15, 20, 25, or about 30 MPa, or any combination of the foregoing values, or a range covering any of the foregoing values. In another respect, the tensile strength may be measured using a tensile test based on ASTM D 412.

[0104] Elongation at break In one respect, the conductive rubber compositions disclosed herein may have an elongation at break greater than about 200%, or from about 200% to about 800%, or about 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, or about 800%, or any combination of the foregoing values, or a range covering any of the foregoing values. In another respect, the elongation at break may be measured using a tensile test based on ASTM D 412.

[0105] Cured or uncured resistors On one hand, the conductive rubber composition disclosed herein can be molded into wires. On the other hand, the wires can be approximately 10 inches (254 mm) long and approximately 2 mm in diameter. In a further aspect, such wires can have an upper limit of approximately 5 ohms (Ω) to approximately 10 megaohms (MΩ), or approximately 5 Ω to approximately 100 kiloohms (kΩ), or approximately 5 Ω, 25 Ω, 50 Ω, 75 Ω, 100 Ω, 200 Ω, 300 Ω, 400 Ω, 500 Ω, 600 Ω, 700 Ω, 800 Ω, or 900 Ω, or 1 kΩ, 5 kΩ, 10 kΩ, 20 kΩ, 30 kΩ, 40 kΩ, 50 kΩ, 60 kΩ, 70 kΩ, 80 kΩ, 90 kΩ, 100 kΩ, 200 kΩ, 300 kΩ, 400 kΩ, 500 kΩ, 600 kΩ, 700 kΩ, 800 kΩ, or 900 kΩ, or 1 MΩ, 2 MΩ, 3 MΩ, 4 The resistivity is MΩ, 5 MΩ, 6 MΩ, 7 MΩ, 8 MΩ, 9 MΩ, or about 10 MΩ, or any combination of the foregoing values, or a range covering any of the foregoing values, at 23°C, whether cured or uncured. On one hand, the resistance can be measured using a standard multimeter. On the other hand, the conductive rubber composition has a resistivity of less than about 800 Ω⋅m, or about 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, or about 800 Ω⋅m, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0106] On the one hand, when the surface area, particle size, and structure (e.g., porosity) of the carbon component are high, the conductivity and / or resistance of the conductive rubber in the disclosed composition are enhanced.

[0107] T25 and T90 In one respect, the conductive rubber composition disclosed herein may have a T25 measured for 60 minutes at 150°C using a standard test with a rotorless rheometer, which is approximately 1 minute to approximately 30 minutes, or approximately 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or approximately 30 minutes, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0108] On the other hand, the conductive rubber composition disclosed herein may have a T90 measured for 60 minutes at 150°C using a standard test with a rotorless rheometer, which is approximately 5 to approximately 60 minutes, or approximately 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, or approximately 60 minutes, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0109] On the one hand, T25 and T90 can be measured using standard tests using a rubber processing analyzer and / or a rotorless rheometer (in accordance with ASTM D 5289 and / or ISO 6502).

[0110] Zwick rebound On one hand, the conductive rubber composition may have a Zwick rebound at 23°C of about 30 to about 60, or about 30, 35, 40, 45, 50, 55, or about 60, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0111] On the other hand, the conductive rubber composition may have a Zwick rebound at 100°C of about 45 to about 75, or about 45, 50, 55, 60, 65, 70, or about 75, or any combination of the foregoing values, or a range covering any of the foregoing values.

[0112] On the one hand, Zwick rebound can be measured using standard test methods for elastomers and rubber, such as DIN 53512, ISO 4662 for rubber, or BS 903.

[0113] Final torque In one aspect, the disclosed conductive rubber composition has a final torque measured at 150°C for 60 minutes, ranging from about 10 dN⋅m to about 45 dN⋅m, or about 10, 15, 20, 25, 30, 35, 40, or about 45 dN⋅m, or any combination of the foregoing values, or covering a range of the foregoing values. In another aspect, the final torque can be measured using a rotorless rheometer to perform tests according to ASTM D 5289 and / or ISO 6502.

[0114] 2 Reversion time In one aspect, the disclosed conductive rubber composition has a two-point recovery time measured at 150°C for 60 minutes, from about 0.1 minutes to about 40 minutes, or about 0.1, 0.5, 1, 5, 10, 15, 20, 25, 30, 35, or about 40 minutes, or any combination of the foregoing values, or covering a range of any of the foregoing values. In another aspect, the two-point recovery time can be measured using a rotorless rheometer to perform tests according to ASTM D 5289 and / or ISO 6502.

[0115] Exemplary methods for evaluating the properties of the disclosed conductive rubber are provided in the embodiments.

[0116] Articles containing conductive rubber compositions On one hand, this document provides articles comprising the conductive rubber compositions disclosed herein. On the other hand, such articles can be tires, tire chimneys, wires, sensors, hoses, electromagnetic interference shielding gaskets, weather-resistant sealing materials, adhesive articles, or any combination thereof. The conductive rubber compositions described herein exhibit excellent resistive properties while using a relatively small amount of carbon component. The compositions also possess good mechanical properties, which reduce the degradation rate of articles made from them (e.g., tires). Therefore, articles incorporating the conductive compositions described herein possess good electrical and mechanical properties.

[0117] Those skilled in the art will recognize, based on the teachings presented in the foregoing description and related drawings, numerous modifications and other embodiments disclosed herein. Therefore, it is to be understood that this disclosure is not limited to the specific embodiments disclosed, and that modifications and other embodiments are intended to be included within the scope of the appended claims. Those skilled in the art will recognize many variations and adaptive modifications to the aspects described herein. These variations and adaptive modifications are intended to be included in the teachings of this disclosure and are covered by the claims herein.

[0118] Although specific terms are used in this document, they are used only in a general and descriptive sense, and not for restrictive purposes.

[0119] As will be apparent to those skilled in the art upon reading this disclosure, each of the individual embodiments described and illustrated herein has separate components and features that can be readily separated from or combined with features of any of the other several embodiments without departing from the scope or spirit of this disclosure.

[0120] Any method described may proceed in the order of the events described or in any other logically possible order. That is, unless expressly stated otherwise, it is not intended to interpret any method or aspect stated herein as requiring its steps to be performed in a particular order. Therefore, where a method claim in the claim or specification does not specifically state that the steps are subject to a particular order, it is not intended to infer the order in any way. This applies to any possible non-explicit basis of interpretation, including logical content relating to the arrangement of steps or procedures, simple meaning derived from grammatical organization or punctuation, or the number or type of aspects described in the specification.

[0121] All publications mentioned herein are incorporated herein by reference to disclose and describe methods and / or materials relating to the cited publications. Only the disclosures of the publications discussed herein prior to the filing date of this application are provided. Nothing herein should be construed as an admission that the invention is not entitled to any prior art based on such publications. Furthermore, the publication dates provided herein may differ from the actual publication dates, which may require independent verification.

[0122] While aspects of this disclosure may be described and claimed under specific statutory categories (e.g., systems statutory categories), this is merely for convenience, and those skilled in the art will understand that each aspect of this disclosure may be described and claimed under any statutory category.

[0123] It should also be understood that the terminology used herein is for descriptive purposes only and is not intended to be limiting. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the disclosed compositions and methods pertain. It should also be understood that terms, such as those defined in common dictionaries, should be interpreted as having the same meaning as they have in the context of the specification and the relevant field, and should not be interpreted in an idealized or overly formal sense unless expressly defined herein.

[0124] Before describing various aspects of this disclosure, the following definitions are provided and should be used unless otherwise stated. Other terms may be defined elsewhere in this disclosure.

[0125] Having described aspects of this disclosure, the following embodiments typically illustrate other aspects of this disclosure. While aspects of this disclosure have been described in conjunction with the following embodiments and the corresponding text and drawings, it is not intended to limit the aspects of this disclosure to that description. Rather, it is intended to cover all alternatives, modifications, and equivalents that are included within the spirit and scope of this disclosure.

[0126] aspect This disclosure may be described according to the following numbered aspects, which should not be confused with the claims.

[0127] Aspect 1. A conductive rubber composition comprising a rubber component and one or more conductive carbon components, wherein the conductive rubber composition has an uncured or cured resistance of less than about 10 MΩ at 23°C when molded into a wire of about 10 inches (254 mm) in length and 2 mm in diameter.

[0128] Aspect 2. The conductive rubber composition of Aspect 1, wherein the rubber component comprises natural rubber (NR), polyisoprene rubber (IR), styrene-butadiene rubber (SBR), polybutadiene rubber (BR), butyl or halogenated butyl rubber, ethylene propylene rubber (EM), ethylene propylene diene monomer (EPDM), chloroprene rubber (CR), nitrile rubber (NBR), hydrogenated acrylonitrile butadiene rubber (HNBR), silicone rubber (MQ), thermoplastic rubber, or any combination thereof.

[0129] Aspect 3. The conductive rubber composition of aspect 2, wherein the butyl or halogenated butyl rubber comprises isobutylene-isoprene rubber (IIR), brominated isobutylene-isoprene rubber (BIIR), chlorinated isobutylene-isoprene rubber (CIIR), brominated isobutylene-co-p-methylstyrene rubber (BIMS), or any combination thereof.

[0130] Aspect 4. The conductive rubber composition of Aspect 2, wherein the thermoplastic rubber comprises poly(styrene-butadiene-styrene) rubber (SBS), thermoplastic elastomer rubber (TPE), melt-processable rubber (MPR), or any combination thereof.

[0131] Aspect 5. The conductive rubber composition of aspect 4, wherein the thermoplastic elastomer rubber comprises thermoplastic polyurethane rubber (TPU).

[0132] Aspect 6. A conductive rubber composition of any one of Aspects 2-5, wherein the conductive rubber composition comprises a blend of two or more rubber components.

[0133] Aspect 7. A conductive rubber composition according to any of the preceding aspects, wherein said rubber component comprises about 5 × 10⁻⁶ 4 Da up to approximately 3 × 10 7 The molecular weight of Da (M) w ).

[0134] Aspect 8. A conductive rubber composition according to any of the preceding aspects, wherein the rubber component comprises approximately 3 × 10⁻⁶ 5 Da up to approximately 5 × 10 6 The molecular weight of Da (M) w ).

[0135] Aspect 9. A conductive rubber composition of any of the preceding aspects, wherein the rubber component comprises a Mooney viscosity (UML) of about 0.01 to about 150.

[0136] Aspect 10. A conductive rubber composition of any of the preceding aspects, wherein the rubber component comprises a Mooney viscosity of about 2 to about 150 UMS.

[0137] Aspect 11. A conductive rubber composition of any of the preceding aspects, wherein the rubber component comprises a glass transition temperature of about -110°C to about -30°C.

[0138] Aspect 12. A conductive rubber composition of any of the preceding aspects, wherein the rubber component comprises a glass transition temperature of about -75°C to about -30°C.

[0139] Aspect 13. A conductive rubber composition of any of the preceding aspects, wherein the one or more conductive carbon components comprise carbon black, short carbon fibers, graphite powder, graphene powder, or any combination thereof.

[0140] Aspect 14. A conductive rubber composition of any of the preceding aspects, wherein the one or more carbon components are present in an amount of about 20 phr to about 150 phr.

[0141] Aspect 15. The conductive rubber composition of aspect 14, wherein the one or more carbon components are present in an amount of about 30 phr to about 100 phr.

[0142] Aspect 16. The conductive rubber composition of aspect 14, wherein the one or more carbon components are present in an amount of about 40 phr to about 80 phr.

[0143] Aspect 17. A conductive rubber composition of any one of Aspects 13-16, wherein the one or more carbon components comprise carbon black having an average particle size of about 5 nm to about 100 nm.

[0144] Aspect 18. The conductive rubber composition of aspect 17, wherein the one or more carbon components comprise carbon black having an average particle size of about 5 nm to about 50 nm.

[0145] Aspect 19. A conductive rubber composition according to any of the preceding aspects, wherein the rubber component comprises a molecular weight distribution of about 2.1 to about 10 (M). w / M n ).

[0146] Aspect 20. A conductive rubber composition according to any of the preceding aspects, wherein the rubber component comprises a molecular weight distribution of about 3.9 to about 8.2 (M w / Mn ).

[0147] Aspect 21. A conductive rubber composition of any one of Aspects 13-20, wherein the one or more carbon components comprise having a carbon content of about 20 μm. 2 / g to approximately 1700 m 2 / g of BET surface area carbon black.

[0148] Aspect 22. A conductive rubber composition of aspect 21, wherein the one or more carbon components comprises having a content of approximately 50 μm 2 / g to approximately 1500 m 2 / g of BET surface area carbon black.

[0149] Aspect 23. A conductive rubber composition of any one of Aspects 13-22, wherein the one or more carbon components comprise having a molecular weight of approximately 20 μm. 3 / g to approximately 1200 m 3 / g of carbon black based on statistical thickness method (STSA).

[0150] Aspect 24. The conductive rubber composition of aspect 23, wherein the one or more carbon components comprises having a content of approximately 100 μm 3 / g to approximately 300 m 3 / g of carbon black based on statistical thickness method (STSA).

[0151] Aspect 25. A conductive rubber composition of any one of Aspects 13-24, wherein the one or more carbon components comprise carbon black having an oil absorption value (OAN) of about 500 mL / 100 g to about 80 mL / 100 g.

[0152] Aspect 26. The conductive rubber composition of aspect 25, wherein the one or more carbon components comprise carbon black having an oil absorption value (OAN) of about 500 mL / 100 g to about 100 mL / 100 g.

[0153] Aspect 27. A conductive rubber composition of any one of Aspects 13-26, wherein the short carbon fibers comprise carbon fibers, chopped carbon fiber yarns, multi-walled carbon nanotubes (MWCNTs), single-walled carbon nanotubes (SWCNTs), or any combination thereof.

[0154] Aspect 28. The conductive rubber composition of aspect 27, wherein the short carbon fibers have a diameter of about 1 nm to about 1000 nm.

[0155] Aspect 29. The conductive rubber composition of aspect 28, wherein the short carbon fibers have a diameter of about 150 nm to about 600 nm.

[0156] A. A conductive rubber composition of any one of A. 27-29, wherein the short carbon fibers have a thickness of about 1 μm to about 1 × 10⁻⁶. 4 The length is μm.

[0157] Aspect 31. A conductive rubber composition of any one of Aspects 28-30, wherein the short carbon fibers have an average transverse length-to-thickness ratio of about 10:1 to about 10,000:1.

[0158] Aspect 32. A conductive rubber composition of any one of Aspects 13-31, wherein the one or more carbon components comprise a blend of carbon black and graphite powder.

[0159] Aspect 33. A conductive rubber composition of any one of Aspects 13-31, wherein the one or more carbon components comprise a blend of carbon black and graphene powder.

[0160] Aspect 34. A conductive rubber composition of any one of Aspects 13-31, wherein the one or more carbon components comprise a blend of carbon black and short carbon fibers.

[0161] Aspect 35. The conductive rubber composition of aspect 34, wherein, in the blend, the short carbon fibers are from about 5 phr to about 80 phr, and the carbon black is from about 15 phr to about 70 phr.

[0162] Aspect 36. The conductive rubber composition of aspect 34, wherein, in the blend, the short carbon fibers are about 20 phr to about 40 phr, and the carbon black is about 10 phr to about 60 phr.

[0163] Aspect 37. The conductive rubber composition of any of the preceding aspects, further comprising at least one antioxidant, at least one anti-ozone agent, or any combination thereof.

[0164] Aspect 38. The conductive rubber composition of aspect 37, wherein the antioxidant comprises an amine antioxidant, a diphenylamine antioxidant, a polymeric dihydroquinoline, or any combination thereof.

[0165] Aspect 39. The conductive rubber composition of aspect 37 or 38, wherein the antioxidant is present in an amount of about 1 phr to about 2 phr.

[0166] Aspect 40. The conductive rubber composition of any of the preceding aspects, further comprising at least one additional component selected from oil, zinc oxide, fatty acid, sulfur, accelerator, anti-scorching agent or any combination thereof.

[0167] Aspect 41. The conductive rubber composition of aspect 40, wherein the oil comprises aromatic rubber processing oil, paraffinic rubber processing oil, naphthenic rubber processing oil, or any combination thereof.

[0168] Aspect 42. The conductive rubber composition of aspect 40 or 41, wherein the oil is present in an amount of about 4 phr to about 30 phr.

[0169] Aspect 43. The conductive rubber composition of aspect 40, wherein the zinc oxide is present in an amount of about 3 phr.

[0170] Aspect 44. The conductive rubber composition of aspect 40, wherein the fatty acid comprises stearic acid, palmitic acid, oleic acid or any combination thereof.

[0171] Aspect 45. Conductive rubber compositions of aspects 40 or 44, wherein the fatty acid is present in an amount of about 1 phr to about 5 phr.

[0172] Aspect 46. The conductive rubber composition of aspect 40, wherein the sulfur is present in an amount of about 0.5 phr to about 5 phr.

[0173] Aspect 47. The conductive rubber composition of aspect 40, wherein the accelerator comprises sulfenamide.

[0174] Aspect 48. Conductive rubber compositions of aspects 40 or 47, wherein the accelerator is present in an amount of about 0.5 phr to about 5 phr.

[0175] Aspect 49. Aspect 40 of conductive rubber compositions, wherein the anti-scorching agent comprises N-(cyclohexylthio)phthalimide.

[0176] Aspect 50. Conductive rubber composition of aspect 40 or 49, wherein the anti-scorching agent is present in an amount of about 0.05 phr to about 0.5 phr.

[0177] Aspect 51. A conductive rubber composition of any one of Aspects 1-50, wherein the rubber component comprises having a density of approximately 3 × 10⁻⁶. 4 Da up to approximately 3 × 10 7 Natural rubber with a molecular weight of Da and a glass transition temperature of approximately -75°C to approximately -65°C.

[0178] Aspect 52. A conductive rubber composition of any one of Aspects 1-50, wherein the rubber component comprises having a density of approximately 2 × 10⁻⁶. 5 Da up to approximately 8 × 10 5 Synthetic cis-1,4-polyisoprene rubber with a molecular weight of Da, a Mooney viscosity of approximately 75 UML, and a glass transition temperature of approximately -70°C to approximately -60°C.

[0179] 53. A conductive rubber composition according to any one of aspects 1-50, wherein the rubber component comprises having a density of about 1 × 10⁻⁶. 5 Da up to approximately 4 × 10 5 Styrene-butadiene rubber with a molecular weight of Da, a Mooney viscosity of approximately 50 UML, and a glass transition temperature of approximately -60°C to approximately -50°C, produced by emulsion polymerization.

[0180] Aspect 54. A conductive rubber composition of any one of Aspects 1-50, wherein the rubber component comprises having a density of approximately 7 × 10⁻⁶. 4 Da up to approximately 8 × 10 4 Styrene-butadiene rubber with a molecular weight of Da, a Mooney viscosity of approximately 2.6 UML, and a glass transition temperature of approximately -30°C to approximately -20°C is produced by solution polymerization.

[0181] Aspect 55. A conductive rubber composition of any one of Aspects 1-50, wherein the conductive carbon component comprises carbon black having an average particle size of about 5 nm to about 100 nm.

[0182] Aspect 56. A conductive rubber composition of any one of Aspects 1-50, wherein the conductive carbon component comprises an average particle size of about 5 nm to about 50 nm and a particle size of about 20 nm. 2 / g to approximately 1500 m 2 Carbon black with an average surface area of ​​ / g.

[0183] Article 57. A conductive rubber composition of any one of Articles 1-50, wherein the conductive carbon component comprises ASTM N299 grade carbon black and has a diameter of about 1 nm to about 1000 nm and a diameter of about 1 μm to about 1 × 10⁻⁶. 4 Short carbon fibers with a length of μm.

[0184] Aspect 58. A conductive rubber composition of any one of Aspects 1-50, wherein the conductive carbon component comprises carbon black having an oil absorption value of about 100 mL / 100 g and a diameter of about 1 nm to about 1000 nm and a diameter of about 1 μm to about 1 × 10⁻⁶ g. 4 Short carbon fibers with a length of μm.

[0185] Aspect 59. A conductive rubber composition of any one of Aspects 1-50, wherein the conductive carbon component comprises carbon black having an average particle size of about 30 nm and having a diameter of about 1 nm to about 1000 nm and a particle size of about 1 μm to about 1 × 10⁻⁶. 4 Short carbon fibers with a length of μm.

[0186] Aspect 60. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has an uncured storage modulus of about 185 kPa to about 1100 kPa at 15% strain, 100°C and 0.83 Hz.

[0187] Aspect 61. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a storage modulus of about 1.1 MPa to about 4 MPa at 1% strain, 100°C and 11 Hz.

[0188] Aspect 62. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a storage modulus of about 0.8 MPa to about 3 MPa at 10% strain, 100°C and 11 Hz.

[0189] Aspect 63. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a storage modulus of about 0.35 MPa to about 1 MPa at 50% strain, 100°C and 11 Hz.

[0190] Aspect 64. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a 10% modulus of about 0.4 MPa to about 2.5 MPa.

[0191] Aspect 65. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a 50% modulus of about 1.25 MPa to about 3.5 MPa.

[0192] Aspect 66. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a 100% modulus of about 2 MPa to about 5.2 MPa.

[0193] Aspect 67. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a 200% modulus of about 3 MPa to about 12 MPa.

[0194] Aspect 68. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a 300% modulus of about 4 MPa to about 13.5 MPa.

[0195] Aspect 69. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a tensile strength of more than about 2 MPa.

[0196] Aspect 70. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a tensile strength of about 4.5 MPa to about 30 MPa.

[0197] Aspect 71. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has an elongation at break of more than about 200%.

[0198] Aspect 72. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has an elongation at break of about 300% to about 800%.

[0199] Aspect 73. A conductive rubber composition of any of the preceding aspects, wherein, when the conductive rubber composition is cured or uncured, the conductive rubber composition has a resistance of about 5 Ω to about 10 MΩ at 23°C when formed into a wire about 10 inches (254 mm) long and 2 mm in diameter.

[0200] Aspect 74. A conductive rubber composition of any of the preceding aspects, wherein, when the conductive rubber composition is cured or uncured, the conductive rubber composition has a resistance of about 5 Ω to about 100 kΩ at 23°C when formed into a wire about 10 inches (254 mm) long and 2 mm in diameter.

[0201] Aspect 75. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a T25 of about 1 minute to about 30 minutes when measured at 150°C for 60 minutes using a standard test with a rotorless rheometer.

[0202] Aspect 76. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a T90 of about 5 minutes to about 60 minutes when measured at 150°C for 60 minutes using a standard test with a rotorless rheometer.

[0203] Aspect 77. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a Zwick rebound of about 30 to about 60 at 23°C.

[0204] Aspect 78. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a Zwick rebound of about 45 to about 75 at 100°C.

[0205] Aspect 79. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition has a final torque of about 10 dN⋅m to about 45 dN⋅m when measured at 150°C for 60 minutes.

[0206] Aspect 80. A conductive rubber composition of any of the preceding aspects, wherein the conductive rubber composition exhibits a 2 pt recovery time of about 0.1 minutes to about 40 minutes when measured at 150°C for 60 minutes.

[0207] Aspect 81. Articles comprising a conductive rubber composition comprising any one of aspects 1-77.

[0208] Articles of Article 81, wherein the articles of Article 82 include tires, tire chimneys, wires, sensors, hoses, electromagnetic interference shielding gaskets, weather-resistant sealing materials, adhesive articles, or any combination thereof. Example

[0209] The following examples are provided to provide those skilled in the art with a complete disclosure and description of how to prepare and evaluate the compounds, compositions, articles, apparatus, and / or methods claimed herein, and are intended to be purely illustrative of the disclosure and not to limit the scope of the disclosure as the inventors believe it to be theirs. Every effort has been made to ensure the accuracy of figures (e.g., amounts, temperatures, etc.), but some errors and deviations should be taken into account. Unless otherwise stated, parts are by weight, temperatures are in °C or at ambient temperature, and pressures are at or near atmospheric pressure.

[0210] Example 1: Property Analysis and Characterization Procedure The Mooney viscosity (ML) or (MS) was determined at 100°C using the standard test method ASTM D 1646.

[0211] The Rubber Processing Analyzer (RPA) is used to determine the following: uncured storage modulus G' at 15% strain, 100°C and 0.83 Hz; T25; T90; storage modulus G' (1%, 10% and 50%) at 100°C and 11 Hz; and Tanδ (10%) at 100°C and 1 Hz.

[0212] Maximum and minimum torque, delta torque, final torque, 1 pt rise time, T25, T90, and 2 pt return were measured using the standard test method for rotorless rheometer (MDR) for rubber properties (vulcanization using a rotorless curing apparatus) based on standard test methods ASTM D 5289 and ISO 6502. The tests were conducted at 150°C for 60 minutes.

[0213] The 10%, 50%, 100%, 200%, and 300% modulus, tensile strength, and elongation at break were measured using a tensile test (dial C) at 23°C based on the standard test method ASTM D 412.

[0214] The external surface area (STSA) is measured according to the standard test method ASTM D 6556 based on the statistical thickness method.

[0215] The resistance of uncured rubber wire was measured at 23°C using a Fluke 117 true RMS multimeter. A typical wire used for this test is 10 inches (254 mm) long and 2 mm in diameter. In this test, a result of "OL" indicates an open circuit where resistance cannot be measured.

[0216] Zwick rebound at 23°C and 100°C was measured using standard test methods for elastomers and rubber, DIN 53512, ISO 4662 (for rubber) and / or BS903.

[0217] Example 2: Exemplary Composition and Its Properties Exemplary conductive rubber compositions using carbon black as a conductive carbon compound are provided in Table 1. a All quantities are provided in parts per hundred parts of rubber (phr). b TSR20 natural rubber is mainly composed of cis-1,4-polyisoprene and has a temperature resistance of -70℃. g With a maximum impurity of 20%. c RSS natural rubber is #2 ribbed smoked sheet (#2 RSS) natural rubber, with a T value of -70℃. g . d Natsyn2200 is a synthetic cis-1,4-polyisoprene with a T0 of -64°C. g . e PLF1502 is an emulsion-polymerized styrene-butadiene rubber with approximately 23.5% styrene, 12% vinyl, 55% trans, 10% cis, and a T0 of -55°C. g . f Exp SBR is an experimental Li-solution SBR with a T0 of -26°C. g . g Carbon black A is N299 ASTM grade carbon black. h Carbon black C was purchased from Orion Engineered Carbons as part of the PRINTEX XE2B commercial. i The oil is a standard rubber processing oil. j Fatty acids are a mixture of stearic acid, palmitic acid, and oleic acid. k The accelerator is a sulfenamide sulfur curing accelerator.

[0218] Table 2 provides the properties of compositions using carbon black as a conductive carbon compound. a OL (open circuit) indicates that the measurement cannot be completed.

[0219] Table 3 provides exemplary compositions using a combination of carbon black and short carbon fibers as conductive carbon compounds. a All quantities are provided in parts per hundred parts of rubber (phr). b For further information on the components, see the footnotes in Table 1. c Carbon black B was purchased from Cabot Corporation as PROPEL X22. d Short carbon fibers have a diameter of 150-600 nm and a length of more than 1 μm.

[0220] Table 4 provides the properties of compositions using a combination of carbon black and short carbon fibers. a OL (open circuit) indicates that the measurement cannot be completed.

[0221] It should be emphasized that the above embodiments of this disclosure are merely possible implementations proposed for the purpose of clearly understanding the principles of this disclosure. Many variations and modifications can be made to the above embodiments (one or more) without substantially departing from the spirit and principles of this disclosure. All such modifications and variations are intended to be included herein within the scope of this disclosure and are protected by the following claims.

Claims

1. A conductive rubber composition comprising a rubber component and one or more conductive carbon components, wherein the conductive rubber composition has an uncured or cured resistance of less than 10 MΩ at 23°C when molded into a wire of 10 inches (254 mm) length and 2 mm diameter. The one or more conductive carbon components are present in an amount of 40 phr to 150 phr, wherein The conductive carbon component is carbon black; or The conductive carbon component comprises carbon black and graphite powder, graphene powder, or any combination thereof, wherein, The carbon black is 40 phr to 50 phr; or The conductive carbon component comprises a blend of carbon black and short carbon fibers, wherein the short carbon fibers have a density of 5 phr to 80 phr, and the carbon black has a density of 40 phr to 70 phr; wherein the short carbon fibers have a diameter of 1 nm to 1000 nm and a density of 1 μm to 1 × 10⁻⁶. 4 The length in μm Furthermore, the carbon black in the conductive carbon component is selected from PRINTEX XE2B, PROPEL X22, and any combination thereof; The rubber component mentioned above is selected from those with a molecular weight of 3 × 10⁻⁶. 4 Up to 3 × 10 7 Natural rubber with a glass transition temperature of -75℃ to -65℃ and a molecular weight of 2 × 10⁻⁶ 5 Up to 8 × 10 5 A synthetic cis-1,4-polyisoprene rubber with a glass transition temperature of -70℃ to -60℃ and a molecular weight of 1 × 10⁻⁶. 5 Up to 4 × 10 5 Styrene-butadiene rubber, and any combination thereof, produced by emulsion polymerization with a glass transition temperature of -60°C to -50°C.

2. The conductive rubber composition according to claim 1, wherein the conductive rubber composition comprises a blend of two or more rubber components.

3. The conductive rubber composition according to claim 1, wherein the short carbon fibers comprise chopped carbon fiber yarns, multi-walled carbon nanotubes (MWCNTs), single-walled carbon nanotubes (SWCNTs), or any combination thereof.

4. The conductive rubber composition according to claim 1, further comprising at least one additional component selected from antioxidants, anti-ozone agents, oils, zinc oxide, fatty acids, sulfur, accelerators, anti-scorching agents, or any combination thereof.

5. The conductive rubber composition according to claim 1, wherein the conductive rubber composition has a tensile strength of 2 MPa to 30 MPa based on ASTM D 412.

6. The conductive rubber composition of claim 1, wherein the conductive rubber composition has an elongation at break of 200% to 800% based on ASTM D 412.

7. An article comprising the conductive rubber composition according to claim 1.

8. The article of claim 7, wherein the article comprises a tire, wire, sensor, hose, electromagnetic interference shielding gasket, weather-resistant sealing material, adhesive article, or any combination thereof.

Citation Information

Patent Citations

  • Conductive rubber material used for flexible sensor as well as preparation method and application of conductive rubber material

    CN105542246A

  • Conductive rubber material for flexible sensors and preparation method and application thereof

    CN105647030A

  • Novel conductive liquid silicone rubber, preparation method and application thereof

    CN110791103A

  • Flexible electromagnetic shielding material and preparation method thereof

    CN111393725A

  • Improved conductive rubber composition and preparation method thereof

    CN112409657A