Catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction, preparation method and application thereof
By using zero-valent iron and phosphorus co-modified carbon materials as catalysts, the gas-solid phase reaction continuous production of 1,1,1,3-tetrachloropropane was achieved, solving the problem of low efficiency in batch reactor reactions and improving efficiency. production efficiency and reduced energy consumption.
Patent Information
- Application Number
- CN202111550988.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-17
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-12-17
AI Technical Summary
The existing synthesis of 1,1,1,3-tetrachloropropane uses a batch reaction, which has problems such as difficulty in catalyst separation, long production time, and waste of energy consumption, resulting in low production efficiency and is not suitable for industrial mass production.
Zero-valent iron and phosphorus co-modified carbon materials are used as catalysts, and zero-valent iron and phosphate functional groups are loaded through the carbon material carrier to achieve continuous production of gas-solid phase reactions, replacing traditional liquid cocatalysts and directly encapsulated into gas-solid phase immobilizers. The synthesis is carried out in a bed reactor.
The continuous synthesis of 1,1,1,3-tetrachloropropane is achieved, which improves production efficiency, reduces energy consumption, gets rid of the dependence on liquid cocatalyst, and is suitable for industrial mass production.
Smart Images

Figure CN116265097B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst for producing 1,1,1,3-tetrachloropropane, in particular to a catalyst for continuously producing 1,1,1,3-tetrachloropropane by gas-solid phase reaction and a preparation method and application thereof, belonging to the technical field of chemical industry. Background Art
[0002] 1,1,1,3-Tetrachloropropane is an important fine chemical and an important raw material for synthesizing paint removers, degreasing agents and various fluorosilicone products, with huge market potential. The chemical is obtained by catalytic oligomerization reaction with carbon tetrachloride and ethylene as raw materials. Commonly used catalytic systems include: iron powder-ferrous chloride (sub)-alkyl (sub) phosphite, iron powder-alkyl (sub) phosphite, alkyl (sub) phosphite-ferrous chloride (sub)-alkyl nitrile, copper powder-alkyl nitrile, etc. In these systems, the co-catalyst alkyl (sub) phosphite or alkyl nitrile are both liquid substances and are indispensable in the reaction. Therefore, the current synthesis of 1,1,1,3-tetrachloropropane can only be carried out by intermittent kettle reaction. However, intermittent kettle reaction has problems such as difficulty in catalyst separation, long production time, limited single kettle output, and energy consumption waste during heating and cooling. The production efficiency is low and it is not suitable for industrial mass production of products. Therefore, the technical field still lacks a solid catalyst and method for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction. Summary of the invention
[0003] The main purpose of the present invention is to provide a catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction and a preparation method thereof, thereby overcoming the deficiencies in the prior art.
[0004] Another object of the present invention is to provide a method for continuously producing 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0006] An embodiment of the present invention provides a catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction, the catalyst comprising zero-valent iron and phosphorus co-modified carbon material, the zero-valent iron and phosphorus co-modified carbon material comprising a carbon material as a carrier, zero-valent iron as an active component loaded on the carrier, and phosphate functional groups formed on the surface of the carbon material.
[0007] An embodiment of the present invention also provides a method for preparing the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction, which comprises: jointly modifying a carbon material with an iron salt and an organic phosphorus to obtain a catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0008] In some embodiments, the preparation method specifically comprises:
[0009] In an inert atmosphere, heating a first mixture comprising a carbon material and an iron salt, and heating the mixture to 600 to 1000° C. at a heating rate of 5° C. / min to 10° C. / min for 1 to 4 hours to obtain a zero-valent iron-modified carbon material;
[0010] And, in an inert atmosphere, heating a second mixture comprising the zero-valent iron-modified carbon material and organic phosphorus to 600-1000° C. and calcining for 1-4 hours to obtain the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0011] In other embodiments, the preparation method specifically comprises:
[0012] In an inert atmosphere, heating the third mixture comprising the carbon material and the organic phosphorus, and heating the mixture to 600 to 1000° C. at a heating rate of 5° C. / min to 10° C. / min for 1 to 4 hours to obtain a phosphorus-modified carbon material;
[0013] Furthermore, the phosphorus-modified carbon material is fully contacted with a solution containing an iron salt for 4 to 6 hours, and a reducing agent is added in an inert atmosphere to reduce at least the iron ions to zero-valent iron, thereby obtaining the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0014] The embodiment of the present invention also provides the use of the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction in continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0015] Accordingly, an embodiment of the present invention further provides a method for continuously producing 1,1,1,3-tetrachloropropane by gas-solid phase reaction, which comprises:
[0016] Encapsulating the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction in a gas-solid phase fixed bed reaction device to form a catalyst bed;
[0017] Carbon tetrachloride and ethylene reaction raw gas are continuously introduced into the catalyst bed, the reaction raw gas inlet pressure is increased to 0.8-1.2 MPa, the temperature of the catalyst bed is heated to 80-120° C., and 1,1,1,3-tetrachloropropane is obtained through catalytic oligomerization reaction.
[0018] Compared with the prior art, the beneficial effects of the present invention are at least:
[0019] The catalyst provided by the present invention uses carbon material as a carrier, and loads the active component zero-valent iron thereon, replacing the main catalyst iron powder in the existing autoclave reaction; the auxiliary component phosphate functional group is formed on the surface of the carbon material through phosphorus modification, replacing the auxiliary catalyst alkyl phosphate in the existing autoclave reaction, and getting rid of the dependence of the traditional intermittent autoclave reaction on liquid catalyst promoters. Therefore, the present invention integrates the main catalyst (zero-valent iron) and the auxiliary catalyst (phosphate functional group) on the carbon material, which can be used directly as a single solid catalyst for the synthesis of 1,1,1,3-tetrachloropropane. Since the liquid auxiliary catalyst is no longer used, the catalyst can be directly encapsulated in a gas-solid fixed bed reactor, and carbon tetrachloride and ethylene raw materials are continuously introduced, and the continuous synthesis of 1,1,1,3-tetrachloropropane can be achieved under pressurized heating conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 This is a microscopic morphology of the zero-valent iron and phosphorus co-modified activated carbon catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0022] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.
[0023] One aspect of an embodiment of the present invention provides a catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction, which is a zero-valent iron and phosphorus co-modified carbon material, wherein the zero-valent iron and phosphorus co-modified carbon material includes a carbon material as a carrier, zero-valent iron as an active component loaded on the carrier, and phosphate functional groups formed on the surface of the carbon material.
[0024] In some embodiments, the mass content of iron in the catalyst is 1 to 10 wt%, and the mass content of phosphorus is 1 to 10 wt%.
[0025] In some embodiments, the particle size of the zero-valent iron in the catalyst is 2 to 100 nm.
[0026] In some embodiments, the carbon material includes at least one of activated carbon, carbon nanotubes, graphene, etc., but is not limited thereto.
[0027] Another aspect of an embodiment of the present invention also provides a method for preparing a catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction, which comprises: jointly modifying a carbon material with an iron salt and an organic phosphorus to obtain a catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0028] In some embodiments, the synthesis method of the catalyst is as follows:
[0029] In an inert atmosphere, heating a first mixture comprising a carbon material and an iron salt, and heating the mixture to 600 to 1000° C. at a heating rate of 5° C. / min to 10° C. / min for 1 to 4 hours to obtain a zero-valent iron-modified carbon material;
[0030] And, in an inert atmosphere, heating a second mixture comprising the zero-valent iron-modified carbon material and organic phosphorus to 600-1000° C. and calcining for 1-4 hours to obtain the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0031] In some specific embodiments, a synthesis step of the catalyst is as follows:
[0032] (1) mixing a carbon material with an iron salt, heating the mixture in an inert atmosphere at a heating rate of 5°C / min to 10°C / min to 600 to 1000°C, calcining the mixture for 1 to 4 hours, and cooling the mixture to room temperature to obtain a zero-valent iron-modified carbon material;
[0033] (2) The zero-valent iron-modified carbon material obtained in step (1) is mixed with organic phosphorus, heated to 600-1000° C. in an inert atmosphere, calcined for 1-4 hours, and cooled to room temperature to obtain the catalyst.
[0034] In some embodiments, another synthesis method of the catalyst is as follows:
[0035] In an inert atmosphere, heating the third mixture comprising the carbon material and the organic phosphorus, and heating the mixture to 600 to 1000° C. at a heating rate of 5° C. / min to 10° C. / min for 1 to 4 hours to obtain a phosphorus-modified carbon material;
[0036] Furthermore, the phosphorus-modified carbon material is fully contacted with a solution containing an iron salt, and a reducing agent is added in an inert atmosphere to reduce at least the iron ions to zero-valent iron, thereby obtaining the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0037] Further, the reducing agent includes sodium borohydride (NaBH4), potassium borohydride (KBH4), etc., but is not limited thereto.
[0038] In other specific embodiments, another synthesis step of the catalyst is as follows:
[0039] (1) mixing a carbon material with an organic phosphorus, heating in an inert atmosphere at a heating rate of 5°C / min to 10°C / min to 600 to 1000°C, calcining for 1 to 4 hours, and cooling to room temperature to obtain a phosphorus-modified carbon material;
[0040] (2) Immersing the phosphorus-modified carbon material obtained in step (1) in an iron salt solution, adding sodium borohydride or potassium borohydride in an inert atmosphere to reduce the iron ions to zero-valent iron.
[0041] (3) filtering, washing and drying to obtain the catalyst.
[0042] Furthermore, the concentration of the reducing agent such as sodium borohydride or potassium borohydride in the reaction system of step (2) is 0.2 mol / L to 0.4 mol / L.
[0043] In some embodiments, the carbon material includes at least one of activated carbon, carbon nanotubes, graphene, etc., but is not limited thereto.
[0044] In some more specific embodiments, the iron salt includes at least one of ferrous chloride, ferrous nitrate, ferrous sulfate, ferric nitrate nonahydrate, ferric chloride, etc., but is not limited thereto.
[0045] Furthermore, the molar ratio of the carbon material to the iron salt is 11:1 to 112:1.
[0046] Furthermore, the molar ratio of the carbon element in the carbon material or the zero-valent iron-modified carbon material to the phosphorus element in the organic phosphorus is 3:1 to 7:1.
[0047] Furthermore, the concentration of the iron salt in the solution containing the iron salt is 0.1 mol / L to 1.8 mol / L.
[0048] In some more specific embodiments, the organic phosphorus includes at least one of phenyl dichlorophosphine, diphenyl phosphine, triphenyl phosphine, diphenyl p-tolyl phosphine and diphenyl cyclohexyl phosphine, but is not limited thereto.
[0049] Another aspect of the embodiments of the present invention further provides a catalyst prepared by the aforementioned method for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0050] Another aspect of the embodiments of the present invention further provides the use of the aforementioned catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction in continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
[0051] Correspondingly, another aspect of an embodiment of the present invention further provides a method for continuously producing 1,1,1,3-tetrachloropropane by gas-solid phase reaction, which mainly comprises: encapsulating a catalyst in a gas-solid phase fixed bed reactor, continuously introducing carbon tetrachloride and ethylene raw gas at a certain pressure and a certain temperature, and obtaining a 1,1,1,3-tetrachloropropane product by catalytic oligomerization reaction.
[0052] In some specific embodiments, the method specifically comprises:
[0053] Encapsulating the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction in a gas-solid phase fixed bed reaction device to form a catalyst bed;
[0054] Carbon tetrachloride and ethylene reaction raw gas are continuously introduced into the catalyst bed, the reaction raw gas inlet pressure is increased to 0.8-1.2 MPa, the temperature of the catalyst bed is heated to 80-120° C., 1,1,1,3-tetrachloropropane is obtained through catalytic oligomerization reaction, and the 1,1,1,3-tetrachloropropane product is collected at the end of the fixed bed.
[0055] Furthermore, the volume ratio of carbon tetrachloride to ethylene is 1:2 to 2:1.
[0056] In summary, the catalyst of the present invention integrates the active component zero-valent iron and the auxiliary component phosphate functional group on the carbon material carrier, gets rid of the dependence of the traditional intermittent reactor reaction on the liquid catalyst auxiliary agent, and realizes the continuous production of 1,1,1,3-tetrachloropropane in a gas-solid phase fixed bed reactor.
[0057] In order to better illustrate the purpose, technical solution and advantages of the present invention, the technical solution of the present invention will be explained in more detail in combination with several preferred embodiments. The specific embodiments described below are only used to further illustrate and explain the present invention, and are not intended to limit the present invention; all variations associated with or derived from the contents disclosed in the present invention are considered to be within the scope of protection of the present invention.
[0058] Example 1
[0059] Take 50g of activated carbon and 50g of ferric nitrate nonahydrate, heat it to 800℃ at a heating rate of 8℃ / min in a nitrogen atmosphere, and roast it for 3 hours. Cool it to room temperature to obtain zero-valent iron-modified activated carbon, then mix it with 100g of triphenylphosphine, roast it at 900℃ in a nitrogen atmosphere for 3 hours to obtain a zero-valent iron and phosphorus co-modified activated carbon catalyst. Elemental analysis shows that the mass content of iron in the catalyst is 3wt%, the mass content of phosphorus is 8wt%, and the particle size of zero-valent iron is 2 to 100nm. Using high-resolution electron transmission microscopy to observe the microscopic morphology of the catalyst, it can be seen that the zero-valent iron particles embedded in the graphite carbon layer are 13nm in size (such as Figure 1 shown).
[0060] Example 2
[0061] 50 g of graphene was mixed with 20 g of ferric chloride, heated to 1000° C. at a heating rate of 10° C. / min in a nitrogen atmosphere and calcined for 2 hours, then cooled to room temperature to obtain zero-valent iron-modified graphene, and then mixed with 110 g of diphenyl-p-tolylphosphine, and calcined at 900° C. for 3 hours in a nitrogen atmosphere to obtain a zero-valent iron and phosphorus co-modified graphene catalyst. Elemental analysis showed that the mass content of iron in the catalyst was 2 wt%, and the mass content of phosphorus was 4 wt%.
[0062] Example 3
[0063] Take 50g of carbon nanotubes and 200g of phenylphosphine dichloride, mix them, heat them to 1000℃ at a heating rate of 6℃ / min in a nitrogen atmosphere, and calcine them for 1 hour to obtain phosphorus-modified carbon nanotubes, then immerse them in 1L aqueous solution containing 50g of ferrous chloride, adjust the pH to <3 with hydrochloric acid, pass nitrogen, and add 1L aqueous solution containing 50g of sodium borohydride dropwise while stirring, then stir for 4 hours, filter, wash, and dry to obtain a zero-valent iron and phosphorus co-modified carbon nanotube catalyst. Elemental analysis shows that the mass content of iron in the catalyst is 8wt%, and the mass content of phosphorus is 5wt%.
[0064] Example 4
[0065] Take 50g of activated carbon and 50g of ferrous nitrate, heat the temperature to 600℃ at a heating rate of 5℃ / min in a nitrogen atmosphere, and calcine for 1 hour, then cool to room temperature to obtain zero-valent iron-modified activated carbon, and then mix it with 100g of diphenylphosphine, and calcine at 900℃ for 3 hours in a nitrogen atmosphere to obtain a zero-valent iron and phosphorus co-modified activated carbon catalyst. Elemental analysis shows that the mass content of iron in the catalyst is 3wt%, and the mass content of phosphorus is 7wt%.
[0066] Example 5
[0067] 50 g of graphene was mixed with 20 g of ferrous chloride, heated to 1000° C. at a heating rate of 8° C. / min in a nitrogen atmosphere, and calcined for 2 hours, then cooled to room temperature to obtain zero-valent iron-modified graphene. The mixture was then mixed with 110 g of diphenylcyclohexylphosphine and calcined at 1000° C. for 1 hour in a nitrogen atmosphere to obtain a zero-valent iron and phosphorus co-modified graphene catalyst. Elemental analysis showed that the mass content of iron in the catalyst was 2 wt%, and the mass content of phosphorus was 3 wt%.
[0068] Example 6
[0069] Take 50g of carbon nanotubes and 200g of phenylphosphine dichloride, heat them to 600℃ at a heating rate of 5℃ / min in a nitrogen atmosphere, and calcine them for 4 hours to obtain phosphorus-modified carbon nanotubes, then immerse them in 1L aqueous solution containing 50g of ferrous nitrate, adjust the pH to <3 with hydrochloric acid, pass nitrogen, and add 1L aqueous solution containing 50g of potassium borohydride dropwise while stirring, then stir for 6 hours, filter, wash and dry to obtain a zero-valent iron and phosphorus co-modified carbon nanotube catalyst. Elemental analysis shows that the mass content of iron in the catalyst is 8wt%, and the mass content of phosphorus is 6wt%.
[0070] Example 7
[0071] 50 g of graphene was mixed with 20 g of ferrous sulfate, and the mixture was heated to 1000° C. at a heating rate of 10° C. / min in a nitrogen atmosphere and calcined for 2 hours, then cooled to room temperature to obtain zero-valent iron-modified graphene. The mixture was then mixed with 110 g of diphenyl-p-tolylphosphine and calcined at 600° C. in a nitrogen atmosphere for 4 hours to obtain a zero-valent iron and phosphorus co-modified graphene catalyst. Elemental analysis showed that the mass content of iron in the catalyst was 2 wt%, and the mass content of phosphorus was 5 wt%.
[0072] Example 8
[0073] In this embodiment, the gas-solid phase fixed bed reactor adopts an electrically heated tubular reactor with a tube diameter of 10 mm and a length of 0.5 m. The reaction process is as follows:
[0074] (1) 20 g of the zero-valent iron and phosphorus co-modified activated carbon catalyst prepared in Example 1 was loaded into a reaction tube;
[0075] (2) preheating carbon tetrachloride at 85°C and then continuously introducing it into the reaction tube together with ethylene, the volume ratio of carbon tetrachloride to ethylene being 1:1, and the total flow rate being 20 mL / min;
[0076] (3) The intake pressure is adjusted to 0.9 MPa;
[0077] (4) heating the catalyst bed temperature to 100° C.;
[0078] (5) collecting crude 1,1,1,3-tetrachloropropane at the end of the fixed bed;
[0079] Gas chromatography analysis of the product obtained in this example showed that the conversion rate of carbon tetrachloride was 70% and the selectivity of 1,1,1,3-tetrachloropropane was 99%.
[0080] Example 9
[0081] In this embodiment, the gas-solid phase fixed bed reactor adopts an electrically heated tubular reactor with a tube diameter of 10 mm and a length of 0.5 m. The reaction process is as follows:
[0082] (1) 20 g of the zero-valent iron and phosphorus co-modified activated carbon catalyst prepared in Example 1 was loaded into a reaction tube;
[0083] (2) preheating carbon tetrachloride at 85°C and then continuously introducing it into the reaction tube together with ethylene, the volume ratio of carbon tetrachloride to ethylene being 1:2, and the total flow rate being 20 mL / min;
[0084] (3) The intake pressure is adjusted to 0.8 MPa;
[0085] (4) heating the catalyst bed temperature to 100° C.;
[0086] (5) collecting crude 1,1,1,3-tetrachloropropane at the end of the fixed bed;
[0087] The product obtained in this example was analyzed by gas chromatography, and the conversion rate of carbon tetrachloride was 68%, and the selectivity of 1,1,1,3-tetrachloropropane was 98.9%.
[0088] Example 10
[0089] In this embodiment, the gas-solid phase fixed bed reactor adopts an electrically heated tubular reactor with a tube diameter of 10 mm and a length of 0.5 m. The reaction process is as follows:
[0090] (1) 20 g of the zero-valent iron and phosphorus co-modified activated carbon catalyst prepared in Example 1 was loaded into a reaction tube;
[0091] (2) preheating carbon tetrachloride at 85°C and then continuously introducing it into the reaction tube together with ethylene, the volume ratio of carbon tetrachloride to ethylene being 2:1, and the total flow rate being 20 mL / min;
[0092] (3) The intake pressure is adjusted to 1.2 MPa;
[0093] (4) heating the catalyst bed temperature to 100° C.;
[0094] (5) collecting crude 1,1,1,3-tetrachloropropane at the end of the fixed bed;
[0095] The product obtained in this example was analyzed by gas chromatography, and the conversion rate of carbon tetrachloride was 72%, and the selectivity of 1,1,1,3-tetrachloropropane was 99.3%.
[0096] Embodiment 11
[0097] In this embodiment, the gas-solid phase fixed bed reactor adopts an electrically heated tubular reactor with a tube diameter of 10 mm and a length of 0.5 m. The reaction process is as follows:
[0098] (1) 20 g of the zero-valent iron and phosphorus co-modified activated carbon catalyst prepared in Example 1 was loaded into a reaction tube;
[0099] (2) preheating carbon tetrachloride at 85°C and then continuously introducing it into the reaction tube together with ethylene, the volume ratio of carbon tetrachloride to ethylene being 1:1, and the total flow rate being 20 mL / min;
[0100] (3) The intake pressure is adjusted to 0.9 MPa;
[0101] (4) heating the catalyst bed temperature to 80°C;
[0102] (5) collecting crude 1,1,1,3-tetrachloropropane at the end of the fixed bed;
[0103] Gas chromatography analysis of the product obtained in this example showed that the conversion rate of carbon tetrachloride was 67% and the selectivity of 1,1,1,3-tetrachloropropane was 98.4%.
[0104] Example 12
[0105] In this embodiment, the gas-solid phase fixed bed reactor adopts an electrically heated tubular reactor with a tube diameter of 10 mm and a length of 0.5 m. The reaction process is as follows:
[0106] (1) 20 g of the zero-valent iron and phosphorus co-modified activated carbon catalyst prepared in Example 1 was loaded into a reaction tube;
[0107] (2) preheating carbon tetrachloride at 85°C and then continuously introducing it into the reaction tube together with ethylene, the volume ratio of carbon tetrachloride to ethylene being 1:1, and the total flow rate being 20 mL / min;
[0108] (3) The intake pressure is adjusted to 0.9 MPa;
[0109] (4) heating the catalyst bed temperature to 120° C.;
[0110] (5) collecting crude 1,1,1,3-tetrachloropropane at the end of the fixed bed;
[0111] The product obtained in this example was analyzed by gas chromatography, and the conversion rate of carbon tetrachloride was 71%, and the selectivity of 1,1,1,3-tetrachloropropane was 98.8%.
[0112] Example 13
[0113] Using the fixed bed reactor of Example 8, the reaction process is:
[0114] (1) 20 g of the zero-valent iron and phosphorus co-modified carbon nanotube catalyst prepared in Example 3 was loaded into a reaction tube;
[0115] (2) preheating carbon tetrachloride at 85°C and then continuously introducing it into the reaction tube together with ethylene, the volume ratio of carbon tetrachloride to ethylene being 1:1, and the total flow rate being 20 mL / min;
[0116] (3) The intake pressure is adjusted to 1 MPa;
[0117] (4) heating the catalyst bed temperature to 110° C.;
[0118] (5) collecting crude 1,1,1,3-tetrachloropropane at the end of the fixed bed;
[0119] Gas chromatography analysis of the product obtained in this example showed that the conversion rate of carbon tetrachloride was 45% and the selectivity of 1,1,1,3-tetrachloropropane was 97%.
[0120] Embodiment 14
[0121] This example uses the fixed bed reactor of Example 8, and the reaction process is:
[0122] (1) 20 g of the zero-valent iron and phosphorus co-modified activated carbon catalyst prepared in Example 4 was loaded into a reaction tube;
[0123] (2) preheating carbon tetrachloride at 85°C and then continuously introducing it into the reaction tube together with ethylene, the volume ratio of carbon tetrachloride to ethylene being 1:2, and the total flow rate being 20 mL / min;
[0124] (3) The intake pressure is adjusted to 0.8 MPa;
[0125] (4) heating the catalyst bed temperature to 90° C.;
[0126] (5) collecting crude 1,1,1,3-tetrachloropropane at the end of the fixed bed;
[0127] The product obtained in this example was analyzed by gas chromatography, and the conversion rate of carbon tetrachloride was 65%, and the selectivity of 1,1,1,3-tetrachloropropane was 96%.
[0128] Embodiment 15
[0129] This example uses the fixed bed reactor of Example 8, and the reaction process is:
[0130] (1) 20 g of the zero-valent iron and phosphorus co-modified carbon nanotube catalyst prepared in Example 6 was loaded into a reaction tube;
[0131] (2) preheating carbon tetrachloride at 85°C and then continuously introducing it into the reaction tube together with ethylene, the volume ratio of carbon tetrachloride to ethylene being 1:1, and the total flow rate being 20 mL / min;
[0132] (3) The intake pressure is adjusted to 1.2 MPa;
[0133] (4) heating the catalyst bed temperature to 120° C.;
[0134] (5) collecting crude 1,1,1,3-tetrachloropropane at the end of the fixed bed;
[0135] Gas chromatography analysis of the product obtained in this example showed that the conversion rate of carbon tetrachloride was 52% and the selectivity of 1,1,1,3-tetrachloropropane was 98%.
[0136] Example 16
[0137] This example uses the fixed bed reactor of Example 8, and the reaction process is:
[0138] (1) 20 g of the zero-valent iron and phosphorus co-modified carbon nanotube catalyst prepared in Example 6 was loaded into a reaction tube;
[0139] (2) preheating carbon tetrachloride at 85°C and then continuously introducing it into the reaction tube together with ethylene, the volume ratio of carbon tetrachloride to ethylene being 2:1, and the total flow rate being 20 mL / min;
[0140] (3) The intake pressure is adjusted to 1.2 MPa;
[0141] (4) heating the catalyst bed temperature to 120° C.;
[0142] (5) collecting crude 1,1,1,3-tetrachloropropane at the end of the fixed bed;
[0143] Gas chromatography analysis of the product obtained in this example showed that the conversion rate of carbon tetrachloride was 52% and the selectivity of 1,1,1,3-tetrachloropropane was 98%.
[0144] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0145] Comparative Example 1
[0146] The difference between this control example and Example 1 is that no ferric nitrate nonahydrate was added, and only a phosphorus-modified activated carbon catalyst was prepared.
[0147] The phosphorus-modified activated carbon catalyst prepared in this comparative example was used in Example 8, and the conversion rate of carbon tetrachloride was 27%, and the selectivity of 1,1,1,3-tetrachloropropane was 41%.
[0148] Comparative Example 2
[0149] The difference between this control example and Example 1 is that no triphenylphosphine is added, and only a zero-valent iron-modified activated carbon catalyst is prepared.
[0150] The zero-valent iron-modified activated carbon catalyst prepared in this comparative example was used in Example 8, and the conversion rate of carbon tetrachloride was 54%, and the selectivity of 1,1,1,3-tetrachloropropane was 67%.
[0151] Comparative Example 3
[0152] The difference between this comparative example and Example 3 is that no ferrous chloride is added, and only phosphorus-modified carbon nanotube catalyst is prepared.
[0153] The phosphorus-modified carbon nanotube catalyst prepared in this comparative example was used in Example 13, and the conversion rate of carbon tetrachloride was 25%, and the selectivity of 1,1,1,3-tetrachloropropane was 56%.
[0154] Comparative Example 4
[0155] The difference between this comparative example and Example 3 is that no phenylphosphine dichloride was added, and only a zero-valent iron-modified carbon nanotube catalyst was prepared.
[0156] The zero-valent iron-modified carbon nanotube catalyst prepared in this comparative example was used in Example 13, and the conversion rate of carbon tetrachloride was 37%, and the selectivity of 1,1,1,3-tetrachloropropane was 60%.
[0157] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction, characterized in that: It includes a zero-valent iron and phosphorus co-modified carbon material, which includes a carbon material as a carrier, zero-valent iron as an active component loaded on the carrier, and a phosphate functional group formed on the surface of the carbon material. The iron content in the catalyst is 1~10wt%, and the phosphorus content is 1~10wt%.
2. The catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction according to claim 1, characterized in that: The particle size of the zero-valent iron in the catalyst is 2-100 nm.
3. The catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction according to claim 1, characterized in that: The carbon material includes at least one of activated carbon, carbon nanotubes and graphene.
4. The method for preparing a catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction according to any one of claims 1 to 3, characterized in that: include: Carbon materials are modified with iron salts and organic phosphorus to obtain a catalyst for the continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
5. The preparation method according to claim 4, characterized in that: Specifically include: In an inert atmosphere, heating a first mixture comprising a carbon material and an iron salt, and heating the mixture to 600-1000° C. at a heating rate of 5° C. / min-10° C. / min for 1-4 hours to obtain a zero-valent iron-modified carbon material; And, in an inert atmosphere, heating a second mixture comprising the zero-valent iron-modified carbon material and organic phosphorus to 600-1000° C. and calcining for 1-4 hours to obtain the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
6. The preparation method according to claim 4, characterized in that: Specifically include: In an inert atmosphere, heating the third mixture comprising the carbon material and the organic phosphorus, and heating the mixture to 600-1000° C. at a heating rate of 5° C. / min-10° C. / min for 1-4 hours to obtain a phosphorus-modified carbon material; Furthermore, the phosphorus-modified carbon material is fully contacted with a solution containing an iron salt for 4 to 6 hours, and a reducing agent is added in an inert atmosphere to reduce at least the iron ions to zero-valent iron, thereby obtaining the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
7. The preparation method according to claim 6, characterized in that: The reducing agent includes sodium borohydride and / or potassium borohydride.
8. The preparation method according to claim 5 or 6, characterized in that: The molar ratio of the carbon material to the iron salt is 11:1 to 112:1; and / or, the molar ratio of carbon element in the carbon material or zero-valent iron-modified carbon material to phosphorus element in the organic phosphorus is 3:1 to 7:1; And / or, the carbon material includes at least one of activated carbon, carbon nanotubes, and graphene; And / or, the iron salt includes at least one of ferrous chloride, ferrous nitrate, ferrous sulfate, ferric nitrate and ferric chloride; And / or, the concentration of the iron salt in the solution containing the iron salt is 0.1 mol / L to 1.8 mol / L; And / or, the organic phosphorus includes at least one of phenyl dichlorophosphine, diphenyl phosphine, triphenyl phosphine, diphenyl p-tolyl phosphine and diphenyl cyclohexyl phosphine.
9. Use of the catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction according to any one of claims 1 to 3 in continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction.
10. A method for continuously producing 1,1,1,3-tetrachloropropane by gas-solid phase reaction, characterized in that include: The catalyst for continuous production of 1,1,1,3-tetrachloropropane by gas-solid phase reaction according to any one of claims 1 to 3 is encapsulated in a gas-solid phase fixed bed reaction device to form a catalyst bed; Carbon tetrachloride and ethylene reaction raw gas are continuously introduced into the catalyst bed, the reaction raw gas inlet pressure is increased to 0.8-1.2 MPa, the temperature of the catalyst bed is heated to 80-120° C., and 1,1,1,3-tetrachloropropane is obtained through catalytic oligomerization reaction.
11. The method according to claim 10, characterized in that: The volume ratio of carbon tetrachloride to ethylene is 1:2 to 2:1.